General
Property | Temperature | Value |
---|---|---|
Densidad | 20.0 °C | 8.9 g/cm³ Show Material materials with Densidad of 8.9 g/cm³ |
Mecánica
Property | Temperature | Value |
---|---|---|
Dureza Brinell | 20.0 °C | 240 [-] Show Material materials with Dureza Brinell of 240 [-] |
Elongación | 20.0 °C | 40 % Show Material materials with Elongación of 40 % |
Límite elástico Rp 0,2 | 20.0 °C | 320 MPa Show Material materials with Límite elástico Rp 0,2 of 320 MPa |
Límite elástico Rp 1,0 | 20.0 °C | 360 MPa Show Material materials with Límite elástico Rp 1,0 of 360 MPa |
Módulo elástico | 20.0 °C | 213 GPa Show Material materials with Módulo elástico of 213 GPa |
100.0 °C | 209 GPa Show Material materials with Módulo elástico of 209 GPa | |
200.0 °C | 204 GPa Show Material materials with Módulo elástico of 204 GPa | |
300.0 °C | 198 GPa Show Material materials with Módulo elástico of 198 GPa | |
400.0 °C | 193 GPa Show Material materials with Módulo elástico of 193 GPa | |
500.0 °C | 188 GPa Show Material materials with Módulo elástico of 188 GPa | |
600.0 °C | 183 GPa Show Material materials with Módulo elástico of 183 GPa | |
Resistencia a la tracción | 20.0 °C | 720 MPa Show Material materials with Resistencia a la tracción of 720 MPa |
Aplicaciones térmicas
Property | Temperature | Value |
---|---|---|
Calor específico | 20.0 °C | 394 J/(kg·K) Show Material materials with Calor específico of 394 J/(kg·K) |
100.0 °C | 410 J/(kg·K) Show Material materials with Calor específico of 410 J/(kg·K) | |
200.0 °C | 421 J/(kg·K) Show Material materials with Calor específico of 421 J/(kg·K) | |
300.0 °C | 429 J/(kg·K) Show Material materials with Calor específico of 429 J/(kg·K) | |
400.0 °C | 436 J/(kg·K) Show Material materials with Calor específico of 436 J/(kg·K) | |
500.0 °C | 450 J/(kg·K) Show Material materials with Calor específico of 450 J/(kg·K) | |
600.0 °C | 464 J/(kg·K) Show Material materials with Calor específico of 464 J/(kg·K) | |
Coeficiente de dilatación térmica | 100.0 °C | 1.06E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.06E-5 1/K |
200.0 °C | 1.11E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.11E-5 1/K | |
300.0 °C | 1.15E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.15E-5 1/K | |
400.0 °C | 1.19E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.19E-5 1/K | |
500.0 °C | 1.21E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.21E-5 1/K | |
Conductividad térmica | 20.0 °C | 13.1 W/(m·K) Show Material materials with Conductividad térmica of 13.1 W/(m·K) |
100.0 °C | 14.4 W/(m·K) Show Material materials with Conductividad térmica of 14.4 W/(m·K) | |
200.0 °C | 15.9 W/(m·K) Show Material materials with Conductividad térmica of 15.9 W/(m·K) | |
300.0 °C | 17.5 W/(m·K) Show Material materials with Conductividad térmica of 17.5 W/(m·K) | |
400.0 °C | 19 W/(m·K) Show Material materials with Conductividad térmica of 19 W/(m·K) | |
500.0 °C | 20.5 W/(m·K) Show Material materials with Conductividad térmica of 20.5 W/(m·K) | |
600.0 °C | 22 W/(m·K) Show Material materials with Conductividad térmica of 22 W/(m·K) | |
Temperatura máx. de funcionamiento, largo | -196 - 450 °C Show Material materials with Temperatura máx. de funcionamiento, largo of -196 - 450 °C |
Eléctrico
Property | Temperature | Value |
---|---|---|
Resistividad eléctrica | 20.0 °C | 1.3E-6 Ω·m Show Material materials with Resistividad eléctrica of 1.3E-6 Ω·m |
100.0 °C | 1.31E-6 Ω·m Show Material materials with Resistividad eléctrica of 1.31E-6 Ω·m | |
200.0 °C | 1.32E-6 Ω·m Show Material materials with Resistividad eléctrica of 1.32E-6 Ω·m | |
300.0 °C | 1.33E-6 Ω·m Show Material materials with Resistividad eléctrica of 1.33E-6 Ω·m | |
400.0 °C | 1.34E-6 Ω·m Show Material materials with Resistividad eléctrica of 1.34E-6 Ω·m | |
500.0 °C | 1.35E-6 Ω·m Show Material materials with Resistividad eléctrica of 1.35E-6 Ω·m | |
600.0 °C | 1.37E-6 Ω·m Show Material materials with Resistividad eléctrica of 1.37E-6 Ω·m | |
Chemical properties
Property | Value |
---|---|
Aluminio | 0.5 % Show Material materials with Aluminio of 0.5 % |
Azufre | 0.015 % Show Material materials with Azufre of 0.015 % |
Carbono | 0.01 % Show Material materials with Carbono of 0.01 % |
Cobalto | 1 % Show Material materials with Cobalto of 1 % |
Cobre | 0.5 % Show Material materials with Cobre of 0.5 % |
Cromo | 6 - 10 % Show Material materials with Cromo of 6 - 10 % |
Fósforo | 0.02 % Show Material materials with Fósforo of 0.02 % |
Hierro | 5 - 8 % Show Material materials with Hierro of 5 - 8 % |
Manganeso | 1 % Show Material materials with Manganeso of 1 % |
Molibdeno | 21 - 25 % Show Material materials with Molibdeno of 21 - 25 % |
Níquel | 53.9 % Show Material materials with Níquel of 53.9 % |
Silicona | 0.1 % Show Material materials with Silicona of 0.1 % |