General
Property | Temperature | Value | Related Standards |
---|---|---|---|
Densidad | 2.72 g/cm³ Show Material materials with Densidad of 2.72 g/cm³ | EN 573-3 | |
20.0 °C | 2.72 g/cm³ Show Material materials with Densidad of 2.72 g/cm³ | DIN 1725-1, EN 573-3, EN 573-4 |
Mecánica
Property | Value | Comment |
---|---|---|
Coeficiente de Poisson | 0.33 [-] Show Material materials with Coeficiente de Poisson of 0.33 [-] | Typical for Wrought 7000 Series Aluminium |
Módulo de cizallamiento | 26.4 - 27.1 GPa Show Material materials with Módulo de cizallamiento of 26.4 - 27.1 GPa | Typical for Wrought 7000 Series Aluminium |
Módulo elástico | 69.0 - 72.0 GPa Show Material materials with Módulo elástico of 69.0 - 72.0 GPa | Typical for Wrought 7000 Series Aluminium |
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 7000 Series Aluminium |
Aplicaciones térmicas
Property | Temperature | Value | Related Standards | Comment |
---|---|---|---|---|
Calor específico | 795.0 - 1050.0 J/(kg·K) Show Material materials with Calor específico of 795.0 - 1050.0 J/(kg·K) | Typical for Wrought 7000 Series Aluminium | ||
Coeficiente de dilatación térmica | 100.0 °C | 2.36e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.36e-05 1/K | DIN 1725-1, EN 573-3, EN 573-4 | |
Conductividad térmica | 20.0 °C | 122.0 W/(m·K) Show Material materials with Conductividad térmica of 122.0 W/(m·K) | DIN 1725-1, EN 573-3, EN 573-4 | |
Temperatura de fusión | 465.0 - 655.0 °C Show Material materials with Temperatura de fusión of 465.0 - 655.0 °C | Typical for Wrought 7000 Series Aluminium |
Eléctrico
Property | Value | Comment |
---|---|---|
Conductividad eléctrica | 18000000.0 - 34000000.0 S/m Show Material materials with Conductividad eléctrica of 18000000.0 - 34000000.0 S/m | Typical for Wrought 7000 Series Aluminium |
Resistividad eléctrica | 2.9e-08 - 5.6e-08 Ω·m Show Material materials with Resistividad eléctrica of 2.9e-08 - 5.6e-08 Ω·m | Typical for Wrought 7000 Series Aluminium |
Chemical properties
Property | Value | Related Standards |
---|---|---|
Cobre | 0.1 % Show Material materials with Cobre of 0.1 % | DIN 1725-1, EN 573-3, EN 573-4 |
Magnesio | 0.1 % Show Material materials with Magnesio of 0.1 % | DIN 1725-1, EN 573-3, EN 573-4 |
Manganeso | 0.1 % Show Material materials with Manganeso of 0.1 % | DIN 1725-1, EN 573-3, EN 573-4 |
Zinc | 0.8 - 1.3 % Show Material materials with Zinc of 0.8 - 1.3 % | DIN 1725-1, EN 573-3, EN 573-4 |
Technological properties
Property | ||
---|---|---|
Brazing | Excellent |