General
Property | Temperature | Value | Condition | Related Standards |
---|---|---|---|---|
Densidad | 20.0 °C | 2.71 g/cm³ Show Material materials with Densidad of 2.71 g/cm³ | F12 | EN 573-3 |
20.0 °C | 2.71 - 2.72 g/cm³ Show Material materials with Densidad of 2.71 - 2.72 g/cm³ | F12 | EN 573-3 | |
20.0 °C | 2.72 g/cm³ Show Material materials with Densidad of 2.72 g/cm³ | F12 | EN 573-3 |
Mecánica
Property | Temperature | Value | Condition | Related Standards | Comment |
---|---|---|---|---|---|
Coeficiente de Poisson | 20.0 °C | 0.33 [-] Show Material materials with Coeficiente de Poisson of 0.33 [-] | F12 | EN 573-3 | |
Elongación | -196.0 °C | 45.0 % Show Material materials with Elongación of 45.0 % | F12 | EN 573-3 | |
-80.0 °C | 24.0 % Show Material materials with Elongación of 24.0 % | F12 | EN 573-3 | ||
-28.0 °C | 20.0 % Show Material materials with Elongación of 20.0 % | F12 | EN 573-3 | ||
20.0 °C | 20.0 % Show Material materials with Elongación of 20.0 % | F12 | EN 573-3 | ||
100.0 °C | 20.0 % Show Material materials with Elongación of 20.0 % | F12 | EN 573-3 | ||
150.0 °C | 23.0 % Show Material materials with Elongación of 23.0 % | F12 | EN 573-3 | ||
200.0 °C | 26.0 % Show Material materials with Elongación of 26.0 % | F12 | EN 573-3 | ||
260.0 °C | 75.0 % Show Material materials with Elongación of 75.0 % | F12 | EN 573-3 | ||
315.0 °C | 80.0 % Show Material materials with Elongación of 80.0 % | F12 | EN 573-3 | ||
370.0 °C | 85.0 % Show Material materials with Elongación of 85.0 % | F12 | EN 573-3 | ||
Módulo de cizallamiento | 20.0 °C | 24.0 - 26.0 GPa Show Material materials with Módulo de cizallamiento of 24.0 - 26.0 GPa | F12 | EN 573-3 | |
20.0 °C | 24.0 - 25.9 GPa Show Material materials with Módulo de cizallamiento of 24.0 - 25.9 GPa | F12 | EN 573-3 | ||
20.0 °C | 25.9 - 26.0 GPa Show Material materials with Módulo de cizallamiento of 25.9 - 26.0 GPa | F12 | EN 573-3 | ||
20.0 °C | 25.9 GPa Show Material materials with Módulo de cizallamiento of 25.9 GPa | F12 | EN 573-3 | ||
Módulo elástico | 20.0 °C | 60.0 - 65.0 GPa Show Material materials with Módulo elástico of 60.0 - 65.0 GPa | F12 | EN 573-3 | |
20.0 °C | 60.0 - 69.0 GPa Show Material materials with Módulo elástico of 60.0 - 69.0 GPa | F12 | EN 573-3 | ||
20.0 °C | 65.0 - 69.0 GPa Show Material materials with Módulo elástico of 65.0 - 69.0 GPa | F12 | EN 573-3 | ||
20.0 °C | 69.0 GPa Show Material materials with Módulo elástico of 69.0 GPa | F12 | EN 573-3 | ||
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 1000 Series Aluminium | |||
Resistencia a la tracción | -196.0 °C | 210.0 MPa Show Material materials with Resistencia a la tracción of 210.0 MPa | F12 | EN 573-3 | |
-80.0 °C | 140.0 MPa Show Material materials with Resistencia a la tracción of 140.0 MPa | F12 | EN 573-3 | ||
-28.0 °C | 130.0 MPa Show Material materials with Resistencia a la tracción of 130.0 MPa | F12 | EN 573-3 | ||
20.0 °C | 125.0 MPa Show Material materials with Resistencia a la tracción of 125.0 MPa | F12 | EN 573-3 | ||
100.0 °C | 110.0 MPa Show Material materials with Resistencia a la tracción of 110.0 MPa | F12 | EN 573-3 | ||
150.0 °C | 95.0 MPa Show Material materials with Resistencia a la tracción of 95.0 MPa | F12 | EN 573-3 | ||
200.0 °C | 70.0 MPa Show Material materials with Resistencia a la tracción of 70.0 MPa | F12 | EN 573-3 | ||
260.0 °C | 30.0 MPa Show Material materials with Resistencia a la tracción of 30.0 MPa | F12 | EN 573-3 | ||
315.0 °C | 20.0 MPa Show Material materials with Resistencia a la tracción of 20.0 MPa | F12 | EN 573-3 | ||
370.0 °C | 15.0 MPa Show Material materials with Resistencia a la tracción of 15.0 MPa | F12 | EN 573-3 |
Aplicaciones térmicas
Property | Temperature | Value | Condition | Related Standards | Comment |
---|---|---|---|---|---|
Calor específico | 20.0 °C | 898.0 J/(kg·K) Show Material materials with Calor específico of 898.0 J/(kg·K) | F12 | EN 573-3 | |
Coeficiente de dilatación térmica | -50.0 °C | 2.17e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.17e-05 1/K | F12 | EN 573-3 | |
100.0 °C | 2.35e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.35e-05 1/K | F12 | EN 573-3 | ||
200.0 °C | 2.44e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.44e-05 1/K | F12 | EN 573-3 | ||
300.0 °C | 2.54e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.54e-05 1/K | F12 | EN 573-3 | ||
Conductividad térmica | 20.0 °C | 205.0 - 210.0 W/(m·K) Show Material materials with Conductividad térmica of 205.0 - 210.0 W/(m·K) | F12 | EN 573-3 | |
20.0 °C | 205.0 - 225.0 W/(m·K) Show Material materials with Conductividad térmica of 205.0 - 225.0 W/(m·K) | F12 | EN 573-3 | ||
20.0 °C | 210.0 - 225.0 W/(m·K) Show Material materials with Conductividad térmica of 210.0 - 225.0 W/(m·K) | F12 | EN 573-3 | ||
20.0 °C | 225.0 W/(m·K) Show Material materials with Conductividad térmica of 225.0 W/(m·K) | F12 | EN 573-3 | ||
Temperatura de fusión | 645.0 - 660.0 °C Show Material materials with Temperatura de fusión of 645.0 - 660.0 °C | Typical for Wrought 1000 Series Aluminium |
Eléctrico
Property | Temperature | Value | Condition | Related Standards |
---|---|---|---|---|
Conductividad eléctrica | 20.0 °C | 34400000.0 - 35500000.0 S/m Show Material materials with Conductividad eléctrica of 34400000.0 - 35500000.0 S/m | F12 | EN 573-3 |
Resistividad eléctrica | 20.0 °C | 2.95e-08 Ω·m Show Material materials with Resistividad eléctrica of 2.95e-08 Ω·m | F12 | EN 573-3 |
Chemical properties
Property | Value | Condition | Related Standards |
---|---|---|---|
Aluminio | 99.0 % Show Material materials with Aluminio of 99.0 % | F12 | EN 573-3 |
Cobre | 0.05 Show Material materials with Cobre of 0.05 | F12 | EN 573-3 |
Manganeso | 0.05 Show Material materials with Manganeso of 0.05 | F12 | EN 573-3 |
Titanio | 0.05 Show Material materials with Titanio of 0.05 | F12 | EN 573-3 |
Zinc | 0.1 Show Material materials with Zinc of 0.1 | F12 | EN 573-3 |
Technological properties
Property | ||
---|---|---|
Brazing | Excellent | |
Workability | Excellent workability. |