General
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Densidad | 2.68 g/cm³ Show Material materials with Densidad of 2.68 g/cm³ | O | EN 573-3, EN 1301, EN 485, EN 13195, EN 754, EN 755 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | |
20.0 °C | 2.68 g/cm³ Show Material materials with Densidad of 2.68 g/cm³ | O | EN 573-3, EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541 | Rod, Flat, Tube, Wire, Sheet | |
20.0 °C | 2.68 - 2.69 g/cm³ Show Material materials with Densidad of 2.68 - 2.69 g/cm³ | O | EN 573-3 | Rod, Flat, Tube, Wire | |
20.0 °C | 2.69 g/cm³ Show Material materials with Densidad of 2.69 g/cm³ | O | EN 573-3 | Rod, Flat, Tube, Wire |
Medidas
Mecánica
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Bending Fatigue Strength | 105.0 MPa Show Material materials with Bending Fatigue Strength of 105.0 MPa | O | EN 573-3, EN 1301, EN 485, EN 754, EN 755 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | ||
Coeficiente de Poisson | 20.0 °C | 0.33 [-] Show Material materials with Coeficiente de Poisson of 0.33 [-] | O | EN 573-3 | Rod, Flat, Tube, Wire | |
Dureza Brinell | 46.0 [-] Show Material materials with Dureza Brinell of 46.0 [-] | O | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | ||
47.0 [-] Show Material materials with Dureza Brinell of 47.0 [-] | O | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | |||
20.0 °C | 45.0 [-] Show Material materials with Dureza Brinell of 45.0 [-] | O | EN 573-3 | Rod, Tube | ||
20.0 °C | 46.0 - 47.0 [-] Show Material materials with Dureza Brinell of 46.0 - 47.0 [-] | O | EN 573-3 | Flat | ||
20.0 °C | 46.0 [-] Show Material materials with Dureza Brinell of 46.0 [-] | O | EN 573-3 | Flat | ||
20.0 °C | 47.0 [-] Show Material materials with Dureza Brinell of 47.0 [-] | O | EN 573-3 | Rod, Tube, Flat | ||
Dureza Brinell (HBW) | 47 [-] Show Material materials with Dureza Brinell (HBW) of 47 [-] | O | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541 | Sheet | ||
Elongación | -196.0 °C | 46.0 % Show Material materials with Elongación of 46.0 % | O | EN 573-3 | ||
-80.0 °C | 35.0 % Show Material materials with Elongación of 35.0 % | O | EN 573-3 | |||
-28.0 °C | 32.0 % Show Material materials with Elongación of 32.0 % | O | EN 573-3 | |||
12.0 % Show Material materials with Elongación of 12.0 % | O | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | A50 | ||
12 % Show Material materials with Elongación of 12 % | O | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541 | Sheet | A50 | ||
14.0 % Show Material materials with Elongación of 14.0 % | O | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | A50 | ||
15.0 % Show Material materials with Elongación of 15.0 % | O | EN 573-3, EN 1301 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | |||
15.0 % Show Material materials with Elongación of 15.0 % | O | EN 573-3, EN 755 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | A50 | ||
16.0 % Show Material materials with Elongación of 16.0 % | O | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | A50 | ||
17.0 % Show Material materials with Elongación of 17.0 % | O | EN 573-3, EN 754 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | A50 | ||
17.0 % Show Material materials with Elongación of 17.0 % | O | EN 573-3, EN 755 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | A100 | ||
18.0 % Show Material materials with Elongación of 18.0 % | O | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | A50 | ||
18.0 % Show Material materials with Elongación of 18.0 % | O | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | A100 | ||
19.0 % Show Material materials with Elongación of 19.0 % | O | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | A50 | ||
20.0 % Show Material materials with Elongación of 20.0 % | O | EN 573-3, EN 754 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | A100 | ||
20.0 °C | 12.0 % Show Material materials with Elongación of 12.0 % | O | EN 573-3 | Flat | A50 | |
20.0 °C | 12.0 % Show Material materials with Elongación of 12.0 % | O | EN 573-3 | Flat | A50 Transverse | |
20.0 °C | 14.0 % Show Material materials with Elongación of 14.0 % | O | EN 573-3 | Flat | A50 | |
20.0 °C | 14.0 % Show Material materials with Elongación of 14.0 % | O | EN 573-3 | Flat | A50 Transverse | |
20.0 °C | 15.0 % Show Material materials with Elongación of 15.0 % | O | EN 573-3 | Rod, Tube | A50 | |
20.0 °C | 15.0 % Show Material materials with Elongación of 15.0 % | O | EN 573-3 | Wire | A100 | |
20.0 °C | 16.0 % Show Material materials with Elongación of 16.0 % | O | EN 573-3 | Flat | A50 | |
20.0 °C | 16.0 % Show Material materials with Elongación of 16.0 % | O | EN 573-3 | Flat | A50 Transverse | |
20.0 °C | 17.0 % Show Material materials with Elongación of 17.0 % | O | EN 573-3 | Rod, Tube | ||
20.0 °C | 17.0 % Show Material materials with Elongación of 17.0 % | O | EN 573-3 | Rod, Tube | A50 | |
20.0 °C | 18.0 % Show Material materials with Elongación of 18.0 % | O | EN 573-3 | Flat | ||
20.0 °C | 18.0 % Show Material materials with Elongación of 18.0 % | O | EN 573-3 | Flat | A50 | |
20.0 °C | 18.0 % Show Material materials with Elongación of 18.0 % | O | EN 573-3 | Flat | A50 Transverse | |
20.0 °C | 18.0 % Show Material materials with Elongación of 18.0 % | O | EN 573-3 | Flat | Transverse | |
20.0 °C | 19.0 % Show Material materials with Elongación of 19.0 % | O | EN 573-3 | Flat | A50 | |
20.0 °C | 19.0 % Show Material materials with Elongación of 19.0 % | O | EN 573-3 | Flat | A50 Transverse | |
20.0 °C | 20.0 % Show Material materials with Elongación of 20.0 % | O | EN 573-3 | Rod, Tube | ||
20.0 °C | 30.0 % Show Material materials with Elongación of 30.0 % | O | EN 573-3 | |||
100.0 °C | 35.0 % Show Material materials with Elongación of 35.0 % | O | EN 573-3 | |||
150.0 °C | 50.0 % Show Material materials with Elongación of 50.0 % | O | EN 573-3 | |||
200.0 °C | 60.0 % Show Material materials with Elongación of 60.0 % | O | EN 573-3 | |||
260.0 °C | 80.0 % Show Material materials with Elongación of 80.0 % | O | EN 573-3 | |||
315.0 °C | 110.0 % Show Material materials with Elongación of 110.0 % | O | EN 573-3 | |||
370.0 °C | 130.0 % Show Material materials with Elongación of 130.0 % | O | EN 573-3 | |||
Límite elástico | -196.0 °C | 110.0 MPa Show Material materials with Límite elástico of 110.0 MPa | O | EN 573-3 | RP02 | |
-80.0 °C | 90.0 MPa Show Material materials with Límite elástico of 90.0 MPa | O | EN 573-3 | RP02 | ||
-28.0 °C | 90.0 MPa Show Material materials with Límite elástico of 90.0 MPa | O | EN 573-3 | RP02 | ||
65.0 MPa Show Material materials with Límite elástico of 65.0 MPa | O | EN 573-3, EN 485, EN 754 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | RP02 | ||
65 MPa Show Material materials with Límite elástico of 65 MPa | O | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541 | Sheet | |||
70.0 MPa Show Material materials with Límite elástico of 70.0 MPa | O | EN 573-3, EN 755 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | RP02 | ||
100.0 MPa Show Material materials with Límite elástico of 100.0 MPa | O | EN 573-3, EN 1301 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | RP02 | ||
20.0 °C | 65.0 MPa Show Material materials with Límite elástico of 65.0 MPa | O | EN 573-3 | Rod, Tube, Flat | RP02 | |
20.0 °C | 65.0 MPa Show Material materials with Límite elástico of 65.0 MPa | O | EN 573-3 | Flat | RP02 Transverse | |
20.0 °C | 70.0 MPa Show Material materials with Límite elástico of 70.0 MPa | O | EN 573-3 | Rod, Tube | RP02 | |
20.0 °C | 90.0 MPa Show Material materials with Límite elástico of 90.0 MPa | O | EN 573-3 | RP02 | ||
20.0 °C | 100.0 MPa Show Material materials with Límite elástico of 100.0 MPa | O | EN 573-3 | Wire | RP02 | |
100.0 °C | 90.0 MPa Show Material materials with Límite elástico of 90.0 MPa | O | EN 573-3 | RP02 | ||
150.0 °C | 90.0 MPa Show Material materials with Límite elástico of 90.0 MPa | O | EN 573-3 | RP02 | ||
200.0 °C | 75.0 MPa Show Material materials with Límite elástico of 75.0 MPa | O | EN 573-3 | RP02 | ||
260.0 °C | 50.0 MPa Show Material materials with Límite elástico of 50.0 MPa | O | EN 573-3 | RP02 | ||
315.0 °C | 40.0 MPa Show Material materials with Límite elástico of 40.0 MPa | O | EN 573-3 | RP02 | ||
370.0 °C | 20.0 MPa Show Material materials with Límite elástico of 20.0 MPa | O | EN 573-3 | RP02 | ||
Módulo de cizallamiento | 26.3 GPa Show Material materials with Módulo de cizallamiento of 26.3 GPa | O | EN 573-3, EN 1301, EN 485, EN 13195, EN 754, EN 755 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | ||
26.5 GPa Show Material materials with Módulo de cizallamiento of 26.5 GPa | O | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541 | Sheet | |||
20.0 °C | 26.3 - 27.0 GPa Show Material materials with Módulo de cizallamiento of 26.3 - 27.0 GPa | O | EN 573-3 | Rod, Flat, Tube, Wire | ||
20.0 °C | 26.3 GPa Show Material materials with Módulo de cizallamiento of 26.3 GPa | O | EN 573-3 | Rod, Flat, Tube, Wire | ||
Módulo elástico | 70.0 GPa Show Material materials with Módulo elástico of 70.0 GPa | O | EN 573-3, EN 1301, EN 485, EN 13195, EN 754, EN 755 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | ||
20.0 °C | 70.0 GPa Show Material materials with Módulo elástico of 70.0 GPa | O | EN 573-3, EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541 | Rod, Flat, Tube, Wire, Sheet | ||
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 5000 Series Aluminium | ||||
Resistencia a la tracción | -196.0 °C | 300.0 MPa Show Material materials with Resistencia a la tracción of 300.0 MPa | O | EN 573-3 | ||
-80.0 °C | 200.0 MPa Show Material materials with Resistencia a la tracción of 200.0 MPa | O | EN 573-3 | |||
-28.0 °C | 195.0 MPa Show Material materials with Resistencia a la tracción of 195.0 MPa | O | EN 573-3 | |||
225.0 MPa Show Material materials with Resistencia a la tracción of 225.0 MPa | O | EN 573-3, EN 1301 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | |||
20.0 °C | 165.0 - 215.0 MPa Show Material materials with Resistencia a la tracción of 165.0 - 215.0 MPa | O | EN 573-3, EN 485 | Flat, Strip, Sheet, Plate, Foil, Wire, Tube, Bar | ||
20.0 °C | 165.0 - 215.0 MPa Show Material materials with Resistencia a la tracción of 165.0 - 215.0 MPa | O | EN 573-3 | Flat | Transverse | |
20.0 °C | 170.0 MPa Show Material materials with Resistencia a la tracción of 170.0 MPa | O | EN 573-3 | Rod | ||
20.0 °C | 170.0 - 230.0 MPa Show Material materials with Resistencia a la tracción of 170.0 - 230.0 MPa | O | EN 573-3, EN 754, EN 755 | Rod, Tube, Strip, Sheet, Plate, Foil, Wire, Bar | ||
20.0 °C | 170.0 - 215.0 MPa Show Material materials with Resistencia a la tracción of 170.0 - 215.0 MPa | O | EN 573-3, EN 485, EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541 | Flat, Strip, Sheet, Plate, Foil, Wire, Tube, Bar | ||
20.0 °C | 170.0 - 215.0 MPa Show Material materials with Resistencia a la tracción of 170.0 - 215.0 MPa | O | EN 573-3 | Flat | Transverse | |
20.0 °C | 195.0 MPa Show Material materials with Resistencia a la tracción of 195.0 MPa | O | EN 573-3 | |||
20.0 °C | 225.0 MPa Show Material materials with Resistencia a la tracción of 225.0 MPa | O | EN 573-3 | Wire | ||
100.0 °C | 195.0 MPa Show Material materials with Resistencia a la tracción of 195.0 MPa | O | EN 573-3 | |||
150.0 °C | 160.0 MPa Show Material materials with Resistencia a la tracción of 160.0 MPa | O | EN 573-3 | |||
200.0 °C | 115.0 MPa Show Material materials with Resistencia a la tracción of 115.0 MPa | O | EN 573-3 | |||
260.0 °C | 85.0 MPa Show Material materials with Resistencia a la tracción of 85.0 MPa | O | EN 573-3 | |||
315.0 °C | 50.0 MPa Show Material materials with Resistencia a la tracción of 50.0 MPa | O | EN 573-3 | |||
370.0 °C | 35.0 MPa Show Material materials with Resistencia a la tracción of 35.0 MPa | O | EN 573-3 | |||
Ángulo de flexión a 180° | 0 °/t Show Material materials with Ángulo de flexión a 180° of 0 °/t | O | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541 | Sheet | ||
0.5 °/t Show Material materials with Ángulo de flexión a 180° of 0.5 °/t | O | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | |||
Ángulo de flexión a 90° | 0 °/t Show Material materials with Ángulo de flexión a 90° of 0 °/t | O | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541 | Sheet | ||
0.5 °/t Show Material materials with Ángulo de flexión a 90° of 0.5 °/t | O | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | |||
1.0 °/t Show Material materials with Ángulo de flexión a 90° of 1.0 °/t | O | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | |||
2.0 °/t Show Material materials with Ángulo de flexión a 90° of 2.0 °/t | O | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar |
Aplicaciones térmicas
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Calor específico | 900.0 J/(kg·K) Show Material materials with Calor específico of 900.0 J/(kg·K) | O | EN 573-3, EN 1301, EN 485, EN 13195, EN 754, EN 755 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | ||
20.0 °C | 900.0 J/(kg·K) Show Material materials with Calor específico of 900.0 J/(kg·K) | O | EN 573-3 | Rod, Flat, Tube, Wire | ||
20.0 °C | 900.0 - 901.0 J/(kg·K) Show Material materials with Calor específico of 900.0 - 901.0 J/(kg·K) | O | EN 573-3 | Rod, Flat, Tube, Wire | ||
20.0 °C | 901.0 J/(kg·K) Show Material materials with Calor específico of 901.0 J/(kg·K) | O | EN 573-3 | Rod, Flat, Tube, Wire | ||
Coeficiente de dilatación térmica | -50.0 °C | 2.21e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.21e-05 1/K | O | EN 573-3 | Rod, Flat, Tube, Wire | |
-50 °C | 2.2100000000000002e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.2100000000000002e-05 1/K | O | EN 573-3, EN 1301, EN 485, EN 13195, EN 754, EN 755 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | ||
20 °C | 2.2100000000000002e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.2100000000000002e-05 1/K | O | EN 573-3, EN 1301, EN 485, EN 13195, EN 754, EN 755 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | ||
20 °C | 2.38e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.38e-05 1/K | O | EN 573-3, EN 1301, EN 485, EN 13195, EN 754, EN 755 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar, Rod, Flat | ||
20 °C | 2.48e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.48e-05 1/K | O | EN 573-3, EN 1301, EN 485, EN 13195, EN 754, EN 755 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar, Rod, Flat | ||
20 °C | 2.5699999999999998e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.5699999999999998e-05 1/K | O | EN 573-3, EN 1301, EN 485, EN 13195, EN 754, EN 755 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | ||
100 °C | 2.38e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.38e-05 1/K | O | EN 573-3, EN 1301, EN 485, EN 13195, EN 754, EN 755 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar, Rod, Flat | ||
100.0 °C | 2.38e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.38e-05 1/K | O | EN 573-3, EN 1301, EN 485, EN 13195, EN 754, EN 755 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar, Rod, Flat | ||
100 °C | 0.000024 1/K Show Material materials with Coeficiente de dilatación térmica of 0.000024 1/K | O | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541 | Sheet | 20-100°C | |
200 °C | 2.48e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.48e-05 1/K | O | EN 573-3, EN 1301, EN 485, EN 13195, EN 754, EN 755 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar, Rod, Flat | ||
200.0 °C | 2.48e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.48e-05 1/K | O | EN 573-3, EN 1301, EN 485, EN 13195, EN 754, EN 755 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar, Rod, Flat | ||
300 °C | 2.5699999999999998e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.5699999999999998e-05 1/K | O | EN 573-3, EN 1301, EN 485, EN 13195, EN 754, EN 755 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | ||
300.0 °C | 2.57e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.57e-05 1/K | O | EN 573-3 | Rod, Flat, Tube, Wire | ||
Conductividad térmica | 138 W/(m·K) Show Material materials with Conductividad térmica of 138 W/(m·K) | O | EN 573-3, EN 1301, EN 485, EN 13195, EN 754, EN 755, EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | ||
20.0 °C | 130.0 - 150.0 W/(m·K) Show Material materials with Conductividad térmica of 130.0 - 150.0 W/(m·K) | O | EN 573-3, EN 1301, EN 485, EN 13195, EN 754, EN 755 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar, Rod, Flat | ||
20.0 °C | 130.0 - 138.0 W/(m·K) Show Material materials with Conductividad térmica of 130.0 - 138.0 W/(m·K) | O | EN 573-3 | Rod, Flat, Tube, Wire | ||
20.0 °C | 138.0 - 150.0 W/(m·K) Show Material materials with Conductividad térmica of 138.0 - 150.0 W/(m·K) | O | EN 573-3 | Rod, Flat, Tube, Wire | ||
20.0 °C | 138.0 W/(m·K) Show Material materials with Conductividad térmica of 138.0 W/(m·K) | O | EN 573-3 | Rod, Flat, Tube, Wire | ||
Temperatura de fusión | 605.0 - 650.0 °C Show Material materials with Temperatura de fusión of 605.0 - 650.0 °C | O | EN 573-3, EN 1301, EN 485, EN 13195, EN 754, EN 755 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | ||
607.0 - 649.0 °C Show Material materials with Temperatura de fusión of 607.0 - 649.0 °C | O | EN 573-3, EN 1301, EN 485, EN 13195, EN 754, EN 755 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | |||
Temperatura máx. de funcionamiento | 150.0 °C Show Material materials with Temperatura máx. de funcionamiento of 150.0 °C | Typical for Wrought 5000 Series Aluminium |
Eléctrico
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Conductividad eléctrica | 20000000.0 S/m Show Material materials with Conductividad eléctrica of 20000000.0 S/m | O | EN 573-3, EN 1301, EN 485, EN 13195, EN 754, EN 755 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | |
20.0 °C | 19000000.0 - 21000000.0 S/m Show Material materials with Conductividad eléctrica of 19000000.0 - 21000000.0 S/m | O | EN 573-3, EN 1301, EN 485, EN 13195, EN 754, EN 755 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar, Rod, Flat | |
Resistividad eléctrica | 4.76e-08 - 5.26e-08 Ω·m Show Material materials with Resistividad eléctrica of 4.76e-08 - 5.26e-08 Ω·m | O | EN 573-3, EN 1301, EN 485, EN 13195, EN 754, EN 755 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | |
4.9e-08 Ω·m Show Material materials with Resistividad eléctrica of 4.9e-08 Ω·m | O | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541 | Sheet | ||
5e-08 Ω·m Show Material materials with Resistividad eléctrica of 5e-08 Ω·m | O | EN 573-3, EN 1301, EN 485, EN 13195, EN 754, EN 755 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | ||
20.0 °C | 4.7e-08 - 4.95e-08 Ω·m Show Material materials with Resistividad eléctrica of 4.7e-08 - 4.95e-08 Ω·m | O | EN 573-3 | Rod, Flat, Tube, Wire | |
20.0 °C | 4.7e-08 - 5.2e-08 Ω·m Show Material materials with Resistividad eléctrica of 4.7e-08 - 5.2e-08 Ω·m | O | EN 573-3 | Rod, Flat, Tube, Wire | |
20.0 °C | 4.95e-08 Ω·m Show Material materials with Resistividad eléctrica of 4.95e-08 Ω·m | O | EN 573-3 | Rod, Flat, Tube, Wire | |
20.0 °C | 4.95e-08 - 5.2e-08 Ω·m Show Material materials with Resistividad eléctrica of 4.95e-08 - 5.2e-08 Ω·m | O | EN 573-3 | Rod, Flat, Tube, Wire |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Cobre | 0.1 % Show Material materials with Cobre of 0.1 % | O | EN 573-3, EN 1301, EN 485, EN 13195, EN 754, EN 755 | Rod, Flat, Tube, Wire, Strip, Sheet, Plate, Foil, Bar |
0.1 % Show Material materials with Cobre of 0.1 % | O | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541 | Sheet | |
Cromo | 0.15 - 0.35 % Show Material materials with Cromo of 0.15 - 0.35 % | O | EN 573-3, EN 1301, EN 485, EN 13195, EN 754, EN 755, EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541 | Rod, Flat, Tube, Wire, Strip, Sheet, Plate, Foil, Bar |
Hierro | 0.4 % Show Material materials with Hierro of 0.4 % | O | EN 573-3 | Rod, Flat, Tube, Wire |
0.40 % Show Material materials with Hierro of 0.40 % | O | EN 573-3, EN 1301, EN 485, EN 13195, EN 754, EN 755 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | |
0.4 % Show Material materials with Hierro of 0.4 % | O | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541 | Sheet | |
Magnesio | 2.2 - 2.8 % Show Material materials with Magnesio of 2.2 - 2.8 % | O | EN 573-3, EN 1301, EN 485, EN 13195, EN 754, EN 755, EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541 | Rod, Flat, Tube, Wire, Strip, Sheet, Plate, Foil, Bar |
Manganeso | 0.1 % Show Material materials with Manganeso of 0.1 % | O | EN 573-3, EN 1301, EN 485, EN 13195, EN 754, EN 755 | Rod, Flat, Tube, Wire, Strip, Sheet, Plate, Foil, Bar |
0.1 % Show Material materials with Manganeso of 0.1 % | O | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541 | Sheet | |
Otro | 0.15 % Show Material materials with Otro of 0.15 % | O | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541 | Sheet |
Silicona | 0.25 % Show Material materials with Silicona of 0.25 % | O | EN 573-3, EN 1301, EN 485, EN 13195, EN 754, EN 755 | Rod, Flat, Tube, Wire, Strip, Sheet, Plate, Foil, Bar |
0.25 % Show Material materials with Silicona of 0.25 % | O | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541 | Sheet | |
Zinc | 0.1 % Show Material materials with Zinc of 0.1 % | O | EN 573-3, EN 1301, EN 485, EN 13195, EN 754, EN 755 | Rod, Flat, Tube, Wire, Strip, Sheet, Plate, Foil, Bar |
0.1 % Show Material materials with Zinc of 0.1 % | O | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541 | Sheet |
Technological properties
Property | ||
---|---|---|
Anodizing | decorative: good, Protective: very good | |
Application areas | Facades: Single sheet, Sheets for composites/ sandwich Panels, Sheets for mechanized panels; Doors: Sheets for composites/ sandwich Panels, Sheets for mechanized panels; Interiors and ceilings: Single sheet, Sheets for composites/ sandwich Panels, Sheets for mechanized panels; Furniture, Plinths, Blinds: Single sheet, Intermediate transformation/interior use; Anodizing quality; Electronic devices: Housing devices; Closures: Easy open; Food can: Body, Lids; Components: Heat shields, Access hatches, Spoilers, General trasportation | |
Corrosion properties | Seawater: very good to good, weathering: good | |
Welding | Very Good | |
Workability | Bending / Spinning (cold): very good / acceptable, Impact extrusion (cold): acceptable, Deep drawing / upsetting (Condition) good (O) / good (H12) |