General
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Densidad | 2.66 g/cm³ Show Material materials with Densidad of 2.66 g/cm³ | O | EN 573-3, EN 13195, EN 14286, EN 1592, EN 485, EN 754, EN 755 | Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire | |
20.0 °C | 2.66 g/cm³ Show Material materials with Densidad of 2.66 g/cm³ | O | EN 573-3, EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Rod, Flat, Seamless Tube, Tube, Coil, Sheet, Plate | |
20.0 °C | 2.66 - 2.67 g/cm³ Show Material materials with Densidad of 2.66 - 2.67 g/cm³ | O | EN 573-3 | Rod, Flat, Seamless Tube, Tube | |
20.0 °C | 2.67 g/cm³ Show Material materials with Densidad of 2.67 g/cm³ | O | EN 573-3 | Rod, Flat, Seamless Tube, Tube |
Medidas
Mecánica
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Bending Fatigue Strength | 120.0 MPa Show Material materials with Bending Fatigue Strength of 120.0 MPa | O | EN 573-3, EN 1592, EN 485, EN 754, EN 755 | Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire | ||
Coeficiente de Poisson | 20.0 °C | 0.33 [-] Show Material materials with Coeficiente de Poisson of 0.33 [-] | O | EN 573-3 | Rod, Flat, Seamless Tube, Tube | |
Dureza Brinell | 65.0 [-] Show Material materials with Dureza Brinell of 65.0 [-] | O | EN 573-3, EN 485 | Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire | ||
20.0 °C | 65.0 [-] Show Material materials with Dureza Brinell of 65.0 [-] | O | EN 573-3 | Rod, Flat, Tube | ||
Dureza Brinell (HBW) | 65 [-] Show Material materials with Dureza Brinell (HBW) of 65 [-] | O | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Coil, Sheet, Plate | ||
Elongación | -196.0 °C | 46.0 % Show Material materials with Elongación of 46.0 % | O | EN 573-3 | ||
-80.0 °C | 35.0 % Show Material materials with Elongación of 35.0 % | O | EN 573-3 | |||
-28.0 °C | 32.0 % Show Material materials with Elongación of 32.0 % | O | EN 573-3 | |||
11.0 % Show Material materials with Elongación of 11.0 % | O | EN 573-3, EN 485 | Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire | A50 | ||
11.0 - 15.0 % Show Material materials with Elongación of 11.0 - 15.0 % | O | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Coil, Sheet, Plate | A50 | ||
12.0 % Show Material materials with Elongación of 12.0 % | O | EN 573-3, EN 485 | Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire | A50 | ||
13.0 % Show Material materials with Elongación of 13.0 % | O | EN 573-3, EN 485 | Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire | A50 | ||
14.0 % Show Material materials with Elongación of 14.0 % | O | EN 573-3, EN 754 | Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire | A50 | ||
15.0 % Show Material materials with Elongación of 15.0 % | O | EN 573-3, EN 485, EN 755 | Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire | A50 | ||
15.0 % Show Material materials with Elongación of 15.0 % | O | EN 573-3, EN 1592 | Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire | A100 | ||
16.0 % Show Material materials with Elongación of 16.0 % | O | EN 573-3, EN 485, EN 754 | Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire | A100 | ||
17.0 % Show Material materials with Elongación of 17.0 % | O | EN 573-3, EN 485 | Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire | A50 | ||
17.0 % Show Material materials with Elongación of 17.0 % | O | EN 573-3, EN 14286 | Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire | A100 | ||
18.0 % Show Material materials with Elongación of 18.0 % | O | EN 573-3, EN 14286, EN 755 | Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire | A100 | ||
20.0 °C | 11.0 % Show Material materials with Elongación of 11.0 % | O | EN 573-3 | Flat | A50 | |
20.0 °C | 11.0 % Show Material materials with Elongación of 11.0 % | O | EN 573-3 | Flat | A50 Transverse | |
20.0 °C | 12.0 % Show Material materials with Elongación of 12.0 % | O | EN 573-3 | Flat | A50 | |
20.0 °C | 12.0 % Show Material materials with Elongación of 12.0 % | O | EN 573-3 | Flat | A50 Transverse | |
20.0 °C | 13.0 % Show Material materials with Elongación of 13.0 % | O | EN 573-3 | Flat | A50 | |
20.0 °C | 13.0 % Show Material materials with Elongación of 13.0 % | O | EN 573-3 | Flat | A50 Transverse | |
20.0 °C | 14.0 % Show Material materials with Elongación of 14.0 % | O | EN 573-3 | Rod, Tube | A50 | |
20.0 °C | 15.0 % Show Material materials with Elongación of 15.0 % | O | EN 573-3 | Seamless Tube | ||
20.0 °C | 15.0 % Show Material materials with Elongación of 15.0 % | O | EN 573-3 | Rod, Tube, Flat | A50 | |
20.0 °C | 15.0 % Show Material materials with Elongación of 15.0 % | O | EN 573-3 | Flat | A50 Transverse | |
20.0 °C | 16.0 % Show Material materials with Elongación of 16.0 % | O | EN 573-3 | Rod, Tube, Flat | ||
20.0 °C | 16.0 % Show Material materials with Elongación of 16.0 % | O | EN 573-3 | Flat | Transverse | |
20.0 °C | 17.0 % Show Material materials with Elongación of 17.0 % | O | EN 573-3 | Flat | A50 | |
20.0 °C | 17.0 % Show Material materials with Elongación of 17.0 % | O | EN 573-3 | Flat | A50 Transverse | |
20.0 °C | 18.0 % Show Material materials with Elongación of 18.0 % | O | EN 573-3 | Rod, Tube | ||
20.0 °C | 30.0 % Show Material materials with Elongación of 30.0 % | O | EN 573-3 | |||
100.0 °C | 36.0 % Show Material materials with Elongación of 36.0 % | O | EN 573-3 | |||
150.0 °C | 50.0 % Show Material materials with Elongación of 50.0 % | O | EN 573-3 | |||
200.0 °C | 60.0 % Show Material materials with Elongación of 60.0 % | O | EN 573-3 | |||
260.0 °C | 80.0 % Show Material materials with Elongación of 80.0 % | O | EN 573-3 | |||
315.0 °C | 110.0 % Show Material materials with Elongación of 110.0 % | O | EN 573-3 | |||
370.0 °C | 130.0 % Show Material materials with Elongación of 130.0 % | O | EN 573-3 | |||
Límite elástico | -196.0 °C | 130.0 MPa Show Material materials with Límite elástico of 130.0 MPa | O | EN 573-3 | RP02 | |
-80.0 °C | 120.0 MPa Show Material materials with Límite elástico of 120.0 MPa | O | EN 573-3 | RP02 | ||
-28.0 °C | 120.0 MPa Show Material materials with Límite elástico of 120.0 MPa | O | EN 573-3 | RP02 | ||
95.0 MPa Show Material materials with Límite elástico of 95.0 MPa | O | EN 573-3, EN 754, EN 755 | Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire | RP02 | ||
100.0 MPa Show Material materials with Límite elástico of 100.0 MPa | O | EN 573-3, EN 14286, EN 1592, EN 485 | Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire | RP02 | ||
100 MPa Show Material materials with Límite elástico of 100 MPa | O | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Coil, Sheet, Plate | |||
20.0 °C | 95.0 MPa Show Material materials with Límite elástico of 95.0 MPa | O | EN 573-3 | Rod, Tube | RP02 | |
20.0 °C | 100.0 MPa Show Material materials with Límite elástico of 100.0 MPa | O | EN 573-3 | Seamless Tube, Flat | RP02 | |
20.0 °C | 100.0 MPa Show Material materials with Límite elástico of 100.0 MPa | O | EN 573-3 | Flat | RP02 Transverse | |
20.0 °C | 120.0 MPa Show Material materials with Límite elástico of 120.0 MPa | O | EN 573-3 | RP02 | ||
100.0 °C | 115.0 MPa Show Material materials with Límite elástico of 115.0 MPa | O | EN 573-3 | RP02 | ||
150.0 °C | 110.0 MPa Show Material materials with Límite elástico of 110.0 MPa | O | EN 573-3 | RP02 | ||
200.0 °C | 105.0 MPa Show Material materials with Límite elástico of 105.0 MPa | O | EN 573-3 | RP02 | ||
260.0 °C | 75.0 MPa Show Material materials with Límite elástico of 75.0 MPa | O | EN 573-3 | RP02 | ||
315.0 °C | 50.0 MPa Show Material materials with Límite elástico of 50.0 MPa | O | EN 573-3 | RP02 | ||
370.0 °C | 30.0 MPa Show Material materials with Límite elástico of 30.0 MPa | O | EN 573-3 | RP02 | ||
Módulo de cizallamiento | 26.7 GPa Show Material materials with Módulo de cizallamiento of 26.7 GPa | O | EN 573-3, EN 13195, EN 14286, EN 1592, EN 485, EN 754, EN 755 | Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire | ||
27.0 GPa Show Material materials with Módulo de cizallamiento of 27.0 GPa | O | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Coil, Sheet, Plate | |||
20.0 °C | 26.7 - 27.0 GPa Show Material materials with Módulo de cizallamiento of 26.7 - 27.0 GPa | O | EN 573-3 | Rod, Flat, Seamless Tube, Tube | ||
20.0 °C | 26.7 GPa Show Material materials with Módulo de cizallamiento of 26.7 GPa | O | EN 573-3 | Rod, Flat, Seamless Tube, Tube | ||
Módulo elástico | 71.0 GPa Show Material materials with Módulo elástico of 71.0 GPa | O | EN 573-3, EN 13195, EN 14286, EN 1592, EN 485, EN 754, EN 755 | Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire | ||
20.0 °C | 71.0 GPa Show Material materials with Módulo elástico of 71.0 GPa | O | EN 573-3, EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Rod, Flat, Seamless Tube, Tube, Coil, Sheet, Plate | ||
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 5000 Series Aluminium | ||||
Resistencia a la tracción | -196.0 °C | 380.0 MPa Show Material materials with Resistencia a la tracción of 380.0 MPa | O | EN 573-3 | ||
-80.0 °C | 270.0 MPa Show Material materials with Resistencia a la tracción of 270.0 MPa | O | EN 573-3 | |||
-28.0 °C | 260.0 MPa Show Material materials with Resistencia a la tracción of 260.0 MPa | O | EN 573-3 | |||
240.0 MPa Show Material materials with Resistencia a la tracción of 240.0 MPa | O | EN 573-3, EN 1592 | Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire | |||
20.0 °C | 240.0 - 320.0 MPa Show Material materials with Resistencia a la tracción of 240.0 - 320.0 MPa | O | EN 573-3, EN 754, EN 755 | Rod, Tube, Strip, Sheet, Plate, Welded Tube, Wire | ||
20.0 °C | 240.0 MPa Show Material materials with Resistencia a la tracción of 240.0 MPa | O | EN 573-3 | Seamless Tube | ||
20.0 °C | 240.0 - 310.0 MPa Show Material materials with Resistencia a la tracción of 240.0 - 310.0 MPa | O | EN 573-3, EN 14286, EN 485, EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Flat, Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire, Coil, Sheet, Plate | ||
20.0 °C | 240.0 - 310.0 MPa Show Material materials with Resistencia a la tracción of 240.0 - 310.0 MPa | O | EN 573-3 | Flat | Transverse | |
20.0 °C | 260.0 MPa Show Material materials with Resistencia a la tracción of 260.0 MPa | O | EN 573-3 | |||
100.0 °C | 260.0 MPa Show Material materials with Resistencia a la tracción of 260.0 MPa | O | EN 573-3 | |||
150.0 °C | 200.0 MPa Show Material materials with Resistencia a la tracción of 200.0 MPa | O | EN 573-3 | |||
200.0 °C | 150.0 MPa Show Material materials with Resistencia a la tracción of 150.0 MPa | O | EN 573-3 | |||
260.0 °C | 115.0 MPa Show Material materials with Resistencia a la tracción of 115.0 MPa | O | EN 573-3 | |||
315.0 °C | 75.0 MPa Show Material materials with Resistencia a la tracción of 75.0 MPa | O | EN 573-3 | |||
370.0 °C | 40.0 MPa Show Material materials with Resistencia a la tracción of 40.0 MPa | O | EN 573-3 | |||
Ángulo de flexión a 180° | 1.0 °/t Show Material materials with Ángulo de flexión a 180° of 1.0 °/t | O | EN 573-3, EN 485 | Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire | ||
1 °/t Show Material materials with Ángulo de flexión a 180° of 1 °/t | O | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Coil, Sheet, Plate | |||
1.5 °/t Show Material materials with Ángulo de flexión a 180° of 1.5 °/t | O | EN 573-3, EN 14286, EN 485 | Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire | |||
3.0 °/t Show Material materials with Ángulo de flexión a 180° of 3.0 °/t | O | EN 573-3, EN 14286 | Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire | |||
Ángulo de flexión a 90° | 0.5 °/t Show Material materials with Ángulo de flexión a 90° of 0.5 °/t | O | EN 573-3, EN 485 | Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire | ||
0.5 °/t Show Material materials with Ángulo de flexión a 90° of 0.5 °/t | O | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Coil, Sheet, Plate | |||
1.0 °/t Show Material materials with Ángulo de flexión a 90° of 1.0 °/t | O | EN 573-3, EN 485 | Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire | |||
1.5 °/t Show Material materials with Ángulo de flexión a 90° of 1.5 °/t | O | EN 573-3, EN 485 | Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire | |||
1.5 °/t Show Material materials with Ángulo de flexión a 90° of 1.5 °/t | O | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Coil, Sheet, Plate | |||
2.5 °/t Show Material materials with Ángulo de flexión a 90° of 2.5 °/t | O | EN 573-3, EN 485 | Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire |
Aplicaciones térmicas
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Calor específico | 900.0 J/(kg·K) Show Material materials with Calor específico of 900.0 J/(kg·K) | O | EN 573-3, EN 13195, EN 14286, EN 1592, EN 485, EN 754, EN 755 | Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire | ||
20.0 °C | 900.0 J/(kg·K) Show Material materials with Calor específico of 900.0 J/(kg·K) | O | EN 573-3 | Rod, Flat, Seamless Tube, Tube | ||
Coeficiente de dilatación térmica | -50 °C | 2.2e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.2e-05 1/K | O | EN 573-3, EN 13195, EN 14286, EN 1592, EN 485, EN 754, EN 755 | Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire, Flat, Seamless Tube | |
-50.0 °C | 2.2e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.2e-05 1/K | O | EN 573-3, EN 13195, EN 14286, EN 1592, EN 485, EN 754, EN 755 | Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire, Flat, Seamless Tube | ||
20 °C | 2.2e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.2e-05 1/K | O | EN 573-3, EN 13195, EN 14286, EN 1592, EN 485, EN 754, EN 755 | Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire, Flat, Seamless Tube | ||
20 °C | 2.38e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.38e-05 1/K | O | EN 573-3, EN 13195, EN 14286, EN 1592, EN 485, EN 754, EN 755 | Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire, Flat, Seamless Tube | ||
20 °C | 2.4699999999999997e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.4699999999999997e-05 1/K | O | EN 573-3, EN 13195, EN 14286, EN 1592, EN 485, EN 754, EN 755 | Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire | ||
20 °C | 2.58e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.58e-05 1/K | O | EN 573-3, EN 13195, EN 14286, EN 1592, EN 485, EN 754, EN 755 | Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire, Flat, Seamless Tube | ||
100 °C | 2.38e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.38e-05 1/K | O | EN 573-3, EN 13195, EN 14286, EN 1592, EN 485, EN 754, EN 755 | Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire, Flat, Seamless Tube | ||
100.0 °C | 2.38e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.38e-05 1/K | O | EN 573-3, EN 13195, EN 14286, EN 1592, EN 485, EN 754, EN 755 | Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire, Flat, Seamless Tube | ||
100 °C | 0.000024 1/K Show Material materials with Coeficiente de dilatación térmica of 0.000024 1/K | O | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Coil, Sheet, Plate | 20-100°C | |
200 °C | 2.4699999999999997e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.4699999999999997e-05 1/K | O | EN 573-3, EN 13195, EN 14286, EN 1592, EN 485, EN 754, EN 755 | Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire | ||
200.0 °C | 2.47e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.47e-05 1/K | O | EN 573-3 | Rod, Flat, Seamless Tube, Tube | ||
300 °C | 2.58e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.58e-05 1/K | O | EN 573-3, EN 13195, EN 14286, EN 1592, EN 485, EN 754, EN 755 | Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire, Flat, Seamless Tube | ||
300.0 °C | 2.58e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.58e-05 1/K | O | EN 573-3, EN 13195, EN 14286, EN 1592, EN 485, EN 754, EN 755 | Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire, Flat, Seamless Tube | ||
Conductividad térmica | 126 W/(m·K) Show Material materials with Conductividad térmica of 126 W/(m·K) | O | EN 573-3, EN 13195, EN 14286, EN 1592, EN 485, EN 754, EN 755, EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire, Coil, Sheet, Plate | ||
20.0 °C | 120.0 - 140.0 W/(m·K) Show Material materials with Conductividad térmica of 120.0 - 140.0 W/(m·K) | O | EN 573-3, EN 13195, EN 14286, EN 1592, EN 485, EN 754, EN 755 | Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire, Flat, Seamless Tube | ||
20.0 °C | 120.0 - 126.0 W/(m·K) Show Material materials with Conductividad térmica of 120.0 - 126.0 W/(m·K) | O | EN 573-3 | Rod, Flat, Seamless Tube, Tube | ||
20.0 °C | 126.0 - 140.0 W/(m·K) Show Material materials with Conductividad térmica of 126.0 - 140.0 W/(m·K) | O | EN 573-3 | Rod, Flat, Seamless Tube, Tube | ||
20.0 °C | 126.0 W/(m·K) Show Material materials with Conductividad térmica of 126.0 W/(m·K) | O | EN 573-3 | Rod, Flat, Seamless Tube, Tube | ||
Temperatura de fusión | 585.0 - 641.0 °C Show Material materials with Temperatura de fusión of 585.0 - 641.0 °C | O | EN 573-3, EN 13195, EN 14286, EN 1592, EN 485, EN 754, EN 755 | Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire | ||
585.0 - 640.0 °C Show Material materials with Temperatura de fusión of 585.0 - 640.0 °C | O | EN 573-3, EN 13195, EN 14286, EN 1592, EN 485, EN 754, EN 755 | Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire | |||
Temperatura máx. de funcionamiento | 150.0 °C Show Material materials with Temperatura máx. de funcionamiento of 150.0 °C | Typical for Wrought 5000 Series Aluminium |
Eléctrico
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Conductividad eléctrica | 18000000.0 S/m Show Material materials with Conductividad eléctrica of 18000000.0 S/m | O | EN 573-3, EN 13195, EN 14286, EN 1592, EN 485, EN 754, EN 755 | Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire | |
20.0 °C | 17000000.0 - 19000000.0 S/m Show Material materials with Conductividad eléctrica of 17000000.0 - 19000000.0 S/m | O | EN 573-3, EN 13195, EN 14286, EN 1592, EN 485, EN 754, EN 755 | Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire, Flat, Seamless Tube | |
Resistividad eléctrica | 5.26e-08 - 5.88e-08 Ω·m Show Material materials with Resistividad eléctrica of 5.26e-08 - 5.88e-08 Ω·m | O | EN 573-3, EN 13195, EN 14286, EN 1592, EN 485, EN 754, EN 755 | Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire | |
5.56e-08 Ω·m Show Material materials with Resistividad eléctrica of 5.56e-08 Ω·m | O | EN 573-3, EN 13195, EN 14286, EN 1592, EN 485, EN 754, EN 755 | Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire | ||
20.0 °C | 5.2e-08 - 5.6e-08 Ω·m Show Material materials with Resistividad eléctrica of 5.2e-08 - 5.6e-08 Ω·m | O | EN 573-3 | Rod, Flat, Seamless Tube, Tube | |
20.0 °C | 5.2e-08 - 5.8e-08 Ω·m Show Material materials with Resistividad eléctrica of 5.2e-08 - 5.8e-08 Ω·m | O | EN 573-3 | Rod, Flat, Seamless Tube, Tube | |
20.0 °C | 5.6e-08 Ω·m Show Material materials with Resistividad eléctrica of 5.6e-08 Ω·m | O | EN 573-3, EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Rod, Flat, Seamless Tube, Tube, Coil, Sheet, Plate | |
20.0 °C | 5.6e-08 - 5.8e-08 Ω·m Show Material materials with Resistividad eléctrica of 5.6e-08 - 5.8e-08 Ω·m | O | EN 573-3 | Rod, Flat, Seamless Tube, Tube |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Cobre | 0.1 % Show Material materials with Cobre of 0.1 % | O | EN 573-3, EN 13195, EN 14286, EN 1592, EN 485, EN 754, EN 755 | Rod, Flat, Seamless Tube, Tube, Strip, Sheet, Plate, Welded Tube, Wire |
0.1 % Show Material materials with Cobre of 0.1 % | O | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Coil, Sheet, Plate | |
Cromo | 0.05 - 0.25 % Show Material materials with Cromo of 0.05 - 0.25 % | O | EN 573-3, EN 13195, EN 14286, EN 1592, EN 485, EN 754, EN 755, EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Rod, Flat, Seamless Tube, Tube, Strip, Sheet, Plate, Welded Tube, Wire, Coil, Sheet, Plate |
Hierro | 0.5 % Show Material materials with Hierro of 0.5 % | O | EN 573-3 | Rod, Flat, Seamless Tube, Tube |
0.50 % Show Material materials with Hierro of 0.50 % | O | EN 573-3, EN 13195, EN 14286, EN 1592, EN 485, EN 754, EN 755 | Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire | |
0.5 % Show Material materials with Hierro of 0.5 % | O | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Coil, Sheet, Plate | |
Magnesio | 3.5 - 4.5 % Show Material materials with Magnesio of 3.5 - 4.5 % | O | EN 573-3, EN 13195, EN 14286, EN 1592, EN 485, EN 754, EN 755, EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Rod, Flat, Seamless Tube, Tube, Strip, Sheet, Plate, Welded Tube, Wire, Coil, Sheet, Plate |
Manganeso | 0.2 - 0.7 % Show Material materials with Manganeso of 0.2 - 0.7 % | O | EN 573-3, EN 13195, EN 14286, EN 1592, EN 485, EN 754, EN 755, EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Rod, Flat, Seamless Tube, Tube, Strip, Sheet, Plate, Welded Tube, Wire, Coil, Sheet, Plate |
Otro | 0.05 - 0.15 % Show Material materials with Otro of 0.05 - 0.15 % | O | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Coil, Sheet, Plate |
Silicona | 0.4 % Show Material materials with Silicona of 0.4 % | O | EN 573-3, EN 13195, EN 14286, EN 1592, EN 485, EN 754, EN 755 | Rod, Flat, Seamless Tube, Tube, Strip, Sheet, Plate, Welded Tube, Wire |
0.4 % Show Material materials with Silicona of 0.4 % | O | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Coil, Sheet, Plate | |
Titanio | 0.15 % Show Material materials with Titanio of 0.15 % | O | EN 573-3, EN 13195, EN 14286, EN 1592, EN 485, EN 754, EN 755 | Rod, Flat, Seamless Tube, Tube, Strip, Sheet, Plate, Welded Tube, Wire |
0.15 % Show Material materials with Titanio of 0.15 % | O | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Coil, Sheet, Plate | |
Zinc | 0.25 % Show Material materials with Zinc of 0.25 % | O | EN 573-3, EN 13195, EN 14286, EN 1592, EN 485, EN 754, EN 755 | Rod, Flat, Seamless Tube, Tube, Strip, Sheet, Plate, Welded Tube, Wire |
0.25 % Show Material materials with Zinc of 0.25 % | O | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Coil, Sheet, Plate |
Technological properties
Property | ||
---|---|---|
Anodizing | decorative: acceptable, Protective: very good | |
Application areas | Vessels: Pressure, Cryogenics; Components: Access hatches, Spoilers, General tranportation | |
Brazing | hard brazing (with flux/ without flux): poor / sufficient, friction soldering: acceptable, soft brazing with flux: poor | |
Corrosion properties | Excellent | |
Welding | Good | |
Workability | Bending / Spinning (cold): good / sufficient, Impact extrusion (cold): sufficient, Deep drawing / upsetting (Condition) good (O) / good (O) |