General
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Densidad | 2.68 g/cm³ Show Material materials with Densidad of 2.68 g/cm³ | H112 | EN 573-3, EN 13195, EN 485, EN 755 | Strip, Sheet, Plate, Rod, Tube | |
20.0 °C | 2.68 g/cm³ Show Material materials with Densidad of 2.68 g/cm³ | H112 | EN 573-3 | Profile, Rod, Flat, Tube, Sheet | |
20.0 °C | 2.68 - 2.69 g/cm³ Show Material materials with Densidad of 2.68 - 2.69 g/cm³ | H112 | EN 573-3 | Profile, Rod, Flat, Tube, Sheet | |
20.0 °C | 2.69 g/cm³ Show Material materials with Densidad of 2.69 g/cm³ | H112 | EN 573-3 | Profile, Rod, Flat, Tube, Sheet |
Mecánica
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Coeficiente de Poisson | 20.0 °C | 0.33 [-] Show Material materials with Coeficiente de Poisson of 0.33 [-] | H112 | EN 573-3 | Profile, Rod, Flat, Tube, Sheet | |
Dureza Brinell | 59.0 [-] Show Material materials with Dureza Brinell of 59.0 [-] | H112 | EN 573-3, EN 485 | Strip, Sheet, Plate, Rod, Tube | ||
63.0 [-] Show Material materials with Dureza Brinell of 63.0 [-] | H112 | EN 573-3, EN 485 | Strip, Sheet, Plate, Rod, Tube | |||
20.0 °C | 59.0 [-] Show Material materials with Dureza Brinell of 59.0 [-] | H112 | EN 573-3 | Sheet, Flat | ||
20.0 °C | 59.0 - 63.0 [-] Show Material materials with Dureza Brinell of 59.0 - 63.0 [-] | H112 | EN 573-3 | Flat | ||
20.0 °C | 60.0 [-] Show Material materials with Dureza Brinell of 60.0 [-] | H112 | EN 573-3 | Profile, Rod, Tube | ||
20.0 °C | 63.0 [-] Show Material materials with Dureza Brinell of 63.0 [-] | H112 | EN 573-3 | Flat | ||
Elongación | 8.0 % Show Material materials with Elongación of 8.0 % | H112 | EN 573-3, EN 485 | Strip, Sheet, Plate, Rod, Tube | A50 | |
9.0 % Show Material materials with Elongación of 9.0 % | H112 | EN 573-3, EN 485 | Strip, Sheet, Plate, Rod, Tube | A100 | ||
13.0 % Show Material materials with Elongación of 13.0 % | H112 | EN 573-3, EN 485 | Strip, Sheet, Plate, Rod, Tube | A100 | ||
14.0 % Show Material materials with Elongación of 14.0 % | H112 | EN 573-3, EN 755 | Strip, Sheet, Plate, Rod, Tube | A50 | ||
16.0 % Show Material materials with Elongación of 16.0 % | H112 | EN 573-3, EN 755 | Strip, Sheet, Plate, Rod, Tube | A100 | ||
20.0 °C | 8.0 % Show Material materials with Elongación of 8.0 % | H112 | EN 573-3 | Flat | A50 | |
20.0 °C | 8.0 % Show Material materials with Elongación of 8.0 % | H112 | EN 573-3 | Flat | A50 Transverse | |
20.0 °C | 9.0 % Show Material materials with Elongación of 9.0 % | H112 | EN 573-3 | Flat | ||
20.0 °C | 9.0 % Show Material materials with Elongación of 9.0 % | H112 | EN 573-3 | Flat | Transverse | |
20.0 °C | 13.0 % Show Material materials with Elongación of 13.0 % | H112 | EN 573-3 | Sheet | ||
20.0 °C | 13.0 % Show Material materials with Elongación of 13.0 % | H112 | EN 573-3 | Flat | Transverse | |
20.0 °C | 14.0 % Show Material materials with Elongación of 14.0 % | H112 | EN 573-3 | Profile, Rod, Tube | A50 | |
20.0 °C | 16.0 % Show Material materials with Elongación of 16.0 % | H112 | EN 573-3 | Profile, Rod, Tube | ||
Módulo de cizallamiento | 26.5 GPa Show Material materials with Módulo de cizallamiento of 26.5 GPa | H112 | EN 573-3, EN 13195, EN 485, EN 755 | Strip, Sheet, Plate, Rod, Tube | ||
20.0 °C | 26.5 - 27.0 GPa Show Material materials with Módulo de cizallamiento of 26.5 - 27.0 GPa | H112 | EN 573-3 | Profile, Rod, Flat, Tube, Sheet | ||
20.0 °C | 26.5 GPa Show Material materials with Módulo de cizallamiento of 26.5 GPa | H112 | EN 573-3 | Profile, Rod, Flat, Tube, Sheet | ||
Módulo elástico | 70.5 GPa Show Material materials with Módulo elástico of 70.5 GPa | H112 | EN 573-3, EN 13195, EN 485, EN 755 | Strip, Sheet, Plate, Rod, Tube | ||
20.0 °C | 70.5 GPa Show Material materials with Módulo elástico of 70.5 GPa | H112 | EN 573-3 | Profile, Rod, Flat, Tube, Sheet | ||
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 5000 Series Aluminium | ||||
Resistencia a la tracción | 200.0 MPa Show Material materials with Resistencia a la tracción of 200.0 MPa | H112 | EN 573-3, EN 755 | Strip, Sheet, Plate, Rod, Tube | ||
215.0 MPa Show Material materials with Resistencia a la tracción of 215.0 MPa | H112 | EN 573-3, EN 485 | Strip, Sheet, Plate, Rod, Tube | |||
220.0 MPa Show Material materials with Resistencia a la tracción of 220.0 MPa | H112 | EN 573-3, EN 485 | Strip, Sheet, Plate, Rod, Tube | |||
20.0 °C | 200.0 MPa Show Material materials with Resistencia a la tracción of 200.0 MPa | H112 | EN 573-3 | Profile, Rod, Tube | ||
20.0 °C | 215.0 MPa Show Material materials with Resistencia a la tracción of 215.0 MPa | H112 | EN 573-3 | Sheet, Flat | ||
20.0 °C | 215.0 MPa Show Material materials with Resistencia a la tracción of 215.0 MPa | H112 | EN 573-3 | Flat | Transverse | |
20.0 °C | 220.0 MPa Show Material materials with Resistencia a la tracción of 220.0 MPa | H112 | EN 573-3 | Flat | ||
20.0 °C | 220.0 MPa Show Material materials with Resistencia a la tracción of 220.0 MPa | H112 | EN 573-3 | Flat | Transverse |
Aplicaciones térmicas
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Calor específico | 900.0 J/(kg·K) Show Material materials with Calor específico of 900.0 J/(kg·K) | H112 | EN 573-3, EN 13195, EN 485, EN 755 | Strip, Sheet, Plate, Rod, Tube | ||
20.0 °C | 897.0 - 900.0 J/(kg·K) Show Material materials with Calor específico of 897.0 - 900.0 J/(kg·K) | H112 | EN 573-3 | Profile, Rod, Flat, Tube, Sheet | ||
20.0 °C | 897.0 J/(kg·K) Show Material materials with Calor específico of 897.0 J/(kg·K) | H112 | EN 573-3 | Profile, Rod, Flat, Tube, Sheet | ||
20.0 °C | 900.0 J/(kg·K) Show Material materials with Calor específico of 900.0 J/(kg·K) | H112 | EN 573-3 | Profile, Rod, Flat, Tube, Sheet | ||
Coeficiente de dilatación térmica | -50 °C | 2.1899999999999997e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.1899999999999997e-05 1/K | H112 | EN 573-3, EN 13195, EN 485, EN 755 | Strip, Sheet, Plate, Rod, Tube | |
-50.0 °C | 2.19e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.19e-05 1/K | H112 | EN 573-3 | Profile, Rod, Flat, Tube, Sheet | ||
20 °C | 2.1899999999999997e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.1899999999999997e-05 1/K | H112 | EN 573-3, EN 13195, EN 485, EN 755 | Strip, Sheet, Plate, Rod, Tube | ||
20 °C | 2.36e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.36e-05 1/K | H112 | EN 573-3, EN 13195, EN 485, EN 755 | Strip, Sheet, Plate, Rod, Tube | ||
20 °C | 2.46e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.46e-05 1/K | H112 | EN 573-3, EN 13195, EN 485, EN 755 | Strip, Sheet, Plate, Rod, Tube, Profile, Flat | ||
20 °C | 2.56e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.56e-05 1/K | H112 | EN 573-3, EN 13195, EN 485, EN 755 | Strip, Sheet, Plate, Rod, Tube, Profile, Flat | ||
100 °C | 2.36e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.36e-05 1/K | H112 | EN 573-3, EN 13195, EN 485, EN 755 | Strip, Sheet, Plate, Rod, Tube | ||
100.0 °C | 2.37e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.37e-05 1/K | H112 | EN 573-3 | Profile, Rod, Flat, Tube, Sheet | ||
200 °C | 2.46e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.46e-05 1/K | H112 | EN 573-3, EN 13195, EN 485, EN 755 | Strip, Sheet, Plate, Rod, Tube, Profile, Flat | ||
200.0 °C | 2.46e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.46e-05 1/K | H112 | EN 573-3, EN 13195, EN 485, EN 755 | Strip, Sheet, Plate, Rod, Tube, Profile, Flat | ||
300 °C | 2.56e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.56e-05 1/K | H112 | EN 573-3, EN 13195, EN 485, EN 755 | Strip, Sheet, Plate, Rod, Tube, Profile, Flat | ||
300.0 °C | 2.56e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.56e-05 1/K | H112 | EN 573-3, EN 13195, EN 485, EN 755 | Strip, Sheet, Plate, Rod, Tube, Profile, Flat | ||
Conductividad térmica | 130.0 - 150.0 W/(m·K) Show Material materials with Conductividad térmica of 130.0 - 150.0 W/(m·K) | H112 | EN 573-3, EN 13195, EN 485, EN 755 | Strip, Sheet, Plate, Rod, Tube | ||
20.0 °C | 135.0 - 150.0 W/(m·K) Show Material materials with Conductividad térmica of 135.0 - 150.0 W/(m·K) | H112 | EN 573-3 | Profile, Rod, Flat, Tube, Sheet | ||
20.0 °C | 135.0 W/(m·K) Show Material materials with Conductividad térmica of 135.0 W/(m·K) | H112 | EN 573-3 | Profile, Rod, Flat, Tube, Sheet | ||
Temperatura de fusión | 602.0 - 646.0 °C Show Material materials with Temperatura de fusión of 602.0 - 646.0 °C | H112 | EN 573-3, EN 13195, EN 485, EN 755 | Strip, Sheet, Plate, Rod, Tube | ||
Temperatura máx. de funcionamiento | 150.0 °C Show Material materials with Temperatura máx. de funcionamiento of 150.0 °C | Typical for Wrought 5000 Series Aluminium |
Eléctrico
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Conductividad eléctrica | 19000000.0 - 21000000.0 S/m Show Material materials with Conductividad eléctrica of 19000000.0 - 21000000.0 S/m | H112 | EN 573-3, EN 13195, EN 485, EN 755 | Strip, Sheet, Plate, Rod, Tube | |
20.0 °C | 21000000.0 S/m Show Material materials with Conductividad eléctrica of 21000000.0 S/m | H112 | EN 573-3 | Profile, Rod, Flat, Tube, Sheet | |
Resistividad eléctrica | 4.76e-08 - 5.26e-08 Ω·m Show Material materials with Resistividad eléctrica of 4.76e-08 - 5.26e-08 Ω·m | H112 | EN 573-3, EN 13195, EN 485, EN 755 | Strip, Sheet, Plate, Rod, Tube | |
20.0 °C | 5.1e-08 Ω·m Show Material materials with Resistividad eléctrica of 5.1e-08 Ω·m | H112 | EN 573-3 | Profile, Rod, Flat, Tube, Sheet |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Cobre | 0.1 % Show Material materials with Cobre of 0.1 % | H112 | EN 573-3, EN 13195, EN 485, EN 755 | Profile, Rod, Flat, Tube, Sheet, Strip, Plate |
Cromo | 0.05 - 0.2 % Show Material materials with Cromo of 0.05 - 0.2 % | H112 | EN 573-3, EN 13195, EN 485, EN 755 | Profile, Rod, Flat, Tube, Sheet, Strip, Plate |
Hierro | 0.4 % Show Material materials with Hierro of 0.4 % | H112 | EN 573-3 | Profile, Rod, Flat, Tube, Sheet |
0.40 % Show Material materials with Hierro of 0.40 % | H112 | EN 573-3, EN 13195, EN 485, EN 755 | Strip, Sheet, Plate, Rod, Tube | |
Magnesio | 2.4 - 3.0 % Show Material materials with Magnesio of 2.4 - 3.0 % | H112 | EN 573-3, EN 13195, EN 485, EN 755 | Profile, Rod, Flat, Tube, Sheet, Strip, Plate |
Manganeso | 0.5 - 1.0 % Show Material materials with Manganeso of 0.5 - 1.0 % | H112 | EN 573-3, EN 13195, EN 485, EN 755 | Profile, Rod, Flat, Tube, Sheet, Strip, Plate |
Silicona | 0.25 % Show Material materials with Silicona of 0.25 % | H112 | EN 573-3, EN 13195, EN 485, EN 755 | Profile, Rod, Flat, Tube, Sheet, Strip, Plate |
Titanio | 0.2 % Show Material materials with Titanio of 0.2 % | H112 | EN 573-3, EN 13195, EN 485, EN 755 | Profile, Rod, Flat, Tube, Sheet, Strip, Plate |
Zinc | 0.25 % Show Material materials with Zinc of 0.25 % | H112 | EN 573-3, EN 13195, EN 485, EN 755 | Profile, Rod, Flat, Tube, Sheet, Strip, Plate |
Technological properties
Property | ||
---|---|---|
Anodizing | decorative: sufficient, Protective: good | |
Brazing | hard brazing (with flux/ without flux): poor / sufficient, friction soldering: acceptable, soft brazing with flux: poor | |
Corrosion properties | Seawater: very good, weathering: very good | |
Workability | Bending / Spinning (cold): good / acceptable, Impact extrusion (cold): sufficient, Deep drawing / upsetting (Condition) good (O) / good (H12) |