General
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Densidad | 2.7 g/cm³ Show Material materials with Densidad of 2.7 g/cm³ | T4 | EN 573-3, EN 1301, EN 1386, EN 1715-3, EN 485, EN 754, EN 755 | Strip, Sheet, Plate, Wire, Tube, Bar | |
20.0 °C | 2.7 g/cm³ Show Material materials with Densidad of 2.7 g/cm³ | T4 | EN 573-3 | Profile, Rod, Flat, Plate, Tube, Wire, Sheet |
Mecánica
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Bending Fatigue Strength | 90.0 MPa Show Material materials with Bending Fatigue Strength of 90.0 MPa | T4 | EN 573-3, EN 1301, EN 1386, EN 1715-3, EN 485, EN 754, EN 755 | Strip, Sheet, Plate, Wire, Tube, Bar | ||
Coeficiente de Poisson | 0.33 [-] Show Material materials with Coeficiente de Poisson of 0.33 [-] | Typical for Wrought 6000 Series Aluminium | ||||
Dureza Brinell | 58.0 [-] Show Material materials with Dureza Brinell of 58.0 [-] | T4 | EN 573-3, EN 485 | Strip, Sheet, Plate, Wire, Tube, Bar | ||
20.0 °C | 58.0 [-] Show Material materials with Dureza Brinell of 58.0 [-] | T4 | EN 573-3 | Flat, Sheet | ||
20.0 °C | 65.0 [-] Show Material materials with Dureza Brinell of 65.0 [-] | T4 | EN 573-3 | Profile, Rod, Tube | ||
Elongación | 6.0 % Show Material materials with Elongación of 6.0 % | T4 | EN 573-3, EN 1386 | Strip, Sheet, Plate, Wire, Tube, Bar | A50 | |
8.0 % Show Material materials with Elongación of 8.0 % | T4 | EN 573-3, EN 1386 | Strip, Sheet, Plate, Wire, Tube, Bar | A50 | ||
10.0 % Show Material materials with Elongación of 10.0 % | T4 | EN 573-3, EN 1386 | Strip, Sheet, Plate, Wire, Tube, Bar | A50 | ||
12.0 % Show Material materials with Elongación of 12.0 % | T4 | EN 573-3, EN 1386, EN 485 | Strip, Sheet, Plate, Wire, Tube, Bar | A50 | ||
13.0 % Show Material materials with Elongación of 13.0 % | T4 | EN 573-3, EN 755 | Strip, Sheet, Plate, Wire, Tube, Bar | A50 | ||
13.0 % Show Material materials with Elongación of 13.0 % | T4 | EN 573-3, EN 1301 | Strip, Sheet, Plate, Wire, Tube, Bar | |||
13.0 % Show Material materials with Elongación of 13.0 % | T4 | EN 573-3, EN 1386 | Strip, Sheet, Plate, Wire, Tube, Bar | A100 | ||
14.0 % Show Material materials with Elongación of 14.0 % | T4 | EN 573-3, EN 485, EN 754 | Strip, Sheet, Plate, Wire, Tube, Bar | A50 | ||
15.0 % Show Material materials with Elongación of 15.0 % | T4 | EN 573-3, EN 755 | Strip, Sheet, Plate, Wire, Tube, Bar | A100 | ||
16.0 % Show Material materials with Elongación of 16.0 % | T4 | EN 573-3, EN 485 | Strip, Sheet, Plate, Wire, Tube, Bar | A50 | ||
16.0 % Show Material materials with Elongación of 16.0 % | T4 | EN 573-3, EN 754 | Strip, Sheet, Plate, Wire, Tube, Bar | A100 | ||
18.0 % Show Material materials with Elongación of 18.0 % | T4 | EN 573-3, EN 485 | Strip, Sheet, Plate, Wire, Tube, Bar | A50 | ||
20.0 °C | 6.0 % Show Material materials with Elongación of 6.0 % | T4 | EN 573-3 | Plate | A50 | |
20.0 °C | 8.0 % Show Material materials with Elongación of 8.0 % | T4 | EN 573-3 | Plate | A50 | |
20.0 °C | 10.0 % Show Material materials with Elongación of 10.0 % | T4 | EN 573-3 | Plate | A50 | |
20.0 °C | 12.0 % Show Material materials with Elongación of 12.0 % | T4 | EN 573-3 | Plate, Flat | A50 | |
20.0 °C | 12.0 % Show Material materials with Elongación of 12.0 % | T4 | EN 573-3 | Flat | A50 Transverse | |
20.0 °C | 13.0 % Show Material materials with Elongación of 13.0 % | T4 | EN 573-3 | Profile, Rod, Tube | A50 | |
20.0 °C | 13.0 % Show Material materials with Elongación of 13.0 % | T4 | EN 573-3 | Plate | ||
20.0 °C | 13.0 % Show Material materials with Elongación of 13.0 % | T4 | EN 573-3 | Wire | A100 | |
20.0 °C | 14.0 % Show Material materials with Elongación of 14.0 % | T4 | EN 573-3 | Rod, Tube, Flat | A50 | |
20.0 °C | 14.0 % Show Material materials with Elongación of 14.0 % | T4 | EN 573-3 | Sheet | ||
20.0 °C | 14.0 % Show Material materials with Elongación of 14.0 % | T4 | EN 573-3 | Flat | A50 Transverse | |
20.0 °C | 14.0 % Show Material materials with Elongación of 14.0 % | T4 | EN 573-3 | Flat | Transverse | |
20.0 °C | 15.0 % Show Material materials with Elongación of 15.0 % | T4 | EN 573-3 | Profile, Rod, Tube, Flat | ||
20.0 °C | 15.0 % Show Material materials with Elongación of 15.0 % | T4 | EN 573-3 | Flat | Transverse | |
20.0 °C | 16.0 % Show Material materials with Elongación of 16.0 % | T4 | EN 573-3 | Flat | A50 | |
20.0 °C | 16.0 % Show Material materials with Elongación of 16.0 % | T4 | EN 573-3 | Rod, Tube | ||
20.0 °C | 16.0 % Show Material materials with Elongación of 16.0 % | T4 | EN 573-3 | Flat | A50 Transverse | |
20.0 °C | 18.0 % Show Material materials with Elongación of 18.0 % | T4 | EN 573-3 | Flat | A50 | |
20.0 °C | 18.0 % Show Material materials with Elongación of 18.0 % | T4 | EN 573-3 | Flat | A50 Transverse | |
Módulo de cizallamiento | 26.3 GPa Show Material materials with Módulo de cizallamiento of 26.3 GPa | T4 | EN 573-3, EN 1301, EN 1386, EN 1715-3, EN 485, EN 754, EN 755 | Strip, Sheet, Plate, Wire, Tube, Bar | ||
20.0 °C | 26.2 GPa Show Material materials with Módulo de cizallamiento of 26.2 GPa | T4 | EN 573-3 | Profile, Rod, Flat, Plate, Tube, Wire, Sheet | ||
Módulo elástico | 69.0 GPa Show Material materials with Módulo elástico of 69.0 GPa | T4 | EN 573-3, EN 1301, EN 1386, EN 1715-3, EN 485, EN 754, EN 755 | Strip, Sheet, Plate, Wire, Tube, Bar | ||
70.0 GPa Show Material materials with Módulo elástico of 70.0 GPa | T4 | EN 573-3, EN 1301, EN 1386, EN 1715-3, EN 485, EN 754, EN 755 | Strip, Sheet, Plate, Wire, Tube, Bar | |||
20.0 °C | 68.3 - 69.6 GPa Show Material materials with Módulo elástico of 68.3 - 69.6 GPa | T4 | EN 573-3 | Profile, Rod, Flat, Plate, Tube, Wire, Sheet | ||
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 6000 Series Aluminium | ||||
Resistencia a la tracción | 180.0 MPa Show Material materials with Resistencia a la tracción of 180.0 MPa | T4 | EN 573-3, EN 755 | Strip, Sheet, Plate, Wire, Tube, Bar | ||
205.0 MPa Show Material materials with Resistencia a la tracción of 205.0 MPa | T4 | EN 573-3, EN 1301, EN 1386, EN 485, EN 754 | Strip, Sheet, Plate, Wire, Tube, Bar | |||
250.0 - 280.0 MPa Show Material materials with Resistencia a la tracción of 250.0 - 280.0 MPa | T4 | EN 573-3, EN 1715-3 | Strip, Sheet, Plate, Wire, Tube, Bar | |||
20.0 °C | 180.0 MPa Show Material materials with Resistencia a la tracción of 180.0 MPa | T4 | EN 573-3 | Profile, Rod, Tube | ||
20.0 °C | 205.0 MPa Show Material materials with Resistencia a la tracción of 205.0 MPa | T4 | EN 573-3 | Rod, Tube, Wire, Sheet, Plate, Flat | ||
20.0 °C | 205.0 MPa Show Material materials with Resistencia a la tracción of 205.0 MPa | T4 | EN 573-3 | Flat | Transverse | |
Ángulo de flexión a 180° | 1.5 °/t Show Material materials with Ángulo de flexión a 180° of 1.5 °/t | T4 | EN 573-3, EN 485 | Strip, Sheet, Plate, Wire, Tube, Bar | ||
2.0 °/t Show Material materials with Ángulo de flexión a 180° of 2.0 °/t | T4 | EN 573-3, EN 485 | Strip, Sheet, Plate, Wire, Tube, Bar | |||
Ángulo de flexión a 90° | 1.0 °/t Show Material materials with Ángulo de flexión a 90° of 1.0 °/t | T4 | EN 573-3, EN 485 | Strip, Sheet, Plate, Wire, Tube, Bar | ||
1.5 °/t Show Material materials with Ángulo de flexión a 90° of 1.5 °/t | T4 | EN 573-3, EN 485 | Strip, Sheet, Plate, Wire, Tube, Bar | |||
3.0 °/t Show Material materials with Ángulo de flexión a 90° of 3.0 °/t | T4 | EN 573-3, EN 485 | Strip, Sheet, Plate, Wire, Tube, Bar | |||
4.0 °/t Show Material materials with Ángulo de flexión a 90° of 4.0 °/t | T4 | EN 573-3, EN 1386, EN 485 | Strip, Sheet, Plate, Wire, Tube, Bar |
Aplicaciones térmicas
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Calor específico | 20.0 °C | 870.0 J/(kg·K) Show Material materials with Calor específico of 870.0 J/(kg·K) | T4 | EN 573-3 | Profile, Rod, Flat, Plate, Tube, Wire, Sheet |
Coeficiente de dilatación térmica | 20 °C | 2.3e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.3e-05 1/K | T4 | EN 573-3, EN 1301, EN 1386, EN 1715-3, EN 485, EN 754, EN 755 | Strip, Sheet, Plate, Wire, Tube, Bar |
20 °C | 2.36e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.36e-05 1/K | T4 | EN 573-3, EN 1301, EN 1386, EN 1715-3, EN 485, EN 754, EN 755 | Strip, Sheet, Plate, Wire, Tube, Bar | |
100 °C | 2.3e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.3e-05 1/K | T4 | EN 573-3, EN 1301, EN 1386, EN 1715-3, EN 485, EN 754, EN 755 | Strip, Sheet, Plate, Wire, Tube, Bar | |
100 °C | 2.36e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.36e-05 1/K | T4 | EN 573-3, EN 1301, EN 1386, EN 1715-3, EN 485, EN 754, EN 755 | Strip, Sheet, Plate, Wire, Tube, Bar | |
Conductividad térmica | 155.0 - 180.0 W/(m·K) Show Material materials with Conductividad térmica of 155.0 - 180.0 W/(m·K) | T4 | EN 573-3, EN 1301, EN 1386, EN 1715-3, EN 485, EN 754, EN 755 | Strip, Sheet, Plate, Wire, Tube, Bar | |
170.0 - 200.0 W/(m·K) Show Material materials with Conductividad térmica of 170.0 - 200.0 W/(m·K) | T4 | EN 573-3, EN 1301, EN 1386, EN 1715-3, EN 485, EN 754, EN 755 | Strip, Sheet, Plate, Wire, Tube, Bar | ||
20.0 °C | 150.0 - 165.0 W/(m·K) Show Material materials with Conductividad térmica of 150.0 - 165.0 W/(m·K) | T4 | EN 573-3 | Profile, Rod, Flat, Plate, Tube, Wire, Sheet | |
Temperatura de fusión | 580.0 - 640.0 °C Show Material materials with Temperatura de fusión of 580.0 - 640.0 °C | T4 | EN 573-3, EN 1301, EN 1386, EN 1715-3, EN 485, EN 754, EN 755 | Strip, Sheet, Plate, Wire, Tube, Bar | |
580.0 - 650.0 °C Show Material materials with Temperatura de fusión of 580.0 - 650.0 °C | T4 | EN 573-3, EN 1301, EN 1386, EN 1715-3, EN 485, EN 754, EN 755 | Strip, Sheet, Plate, Wire, Tube, Bar |
Eléctrico
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Conductividad eléctrica | 22000000.0 - 30000000.0 S/m Show Material materials with Conductividad eléctrica of 22000000.0 - 30000000.0 S/m | T4 | EN 573-3, EN 1301, EN 1386, EN 1715-3, EN 485, EN 754, EN 755 | Strip, Sheet, Plate, Wire, Tube, Bar | |
23000000.0 - 27000000.0 S/m Show Material materials with Conductividad eléctrica of 23000000.0 - 27000000.0 S/m | T4 | EN 573-3, EN 1301, EN 1386, EN 1715-3, EN 485, EN 754, EN 755 | Strip, Sheet, Plate, Wire, Tube, Bar | ||
20.0 °C | 20000000.0 - 30000000.0 S/m Show Material materials with Conductividad eléctrica of 20000000.0 - 30000000.0 S/m | T4 | EN 573-3 | Profile, Rod, Flat, Plate, Tube, Wire, Sheet | |
Resistividad eléctrica | 3.33e-08 - 4.55e-08 Ω·m Show Material materials with Resistividad eléctrica of 3.33e-08 - 4.55e-08 Ω·m | T4 | EN 573-3, EN 1301, EN 1386, EN 1715-3, EN 485, EN 754, EN 755 | Strip, Sheet, Plate, Wire, Tube, Bar | |
3.7e-08 - 4.35e-08 Ω·m Show Material materials with Resistividad eléctrica of 3.7e-08 - 4.35e-08 Ω·m | T4 | EN 573-3, EN 1301, EN 1386, EN 1715-3, EN 485, EN 754, EN 755 | Strip, Sheet, Plate, Wire, Tube, Bar |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Cobre | 0.15 - 0.4 % Show Material materials with Cobre of 0.15 - 0.4 % | T4 | EN 573-3, EN 1301, EN 1386, EN 1715-3, EN 485, EN 754, EN 755 | Profile, Rod, Flat, Plate, Tube, Wire, Sheet, Strip, Bar |
Cromo | 0.04 - 0.35 % Show Material materials with Cromo of 0.04 - 0.35 % | T4 | EN 573-3, EN 1301, EN 1386, EN 1715-3, EN 485, EN 754, EN 755 | Profile, Rod, Flat, Plate, Tube, Wire, Sheet, Strip, Bar |
Hierro | 0.7 % Show Material materials with Hierro of 0.7 % | T4 | EN 573-3 | Profile, Rod, Flat, Plate, Tube, Wire, Sheet |
0.70 % Show Material materials with Hierro of 0.70 % | T4 | EN 573-3, EN 1301, EN 1386, EN 1715-3, EN 485, EN 754, EN 755 | Strip, Sheet, Plate, Wire, Tube, Bar | |
Magnesio | 0.8 - 1.2 % Show Material materials with Magnesio of 0.8 - 1.2 % | T4 | EN 573-3, EN 1301, EN 1386, EN 1715-3, EN 485, EN 754, EN 755 | Profile, Rod, Flat, Plate, Tube, Wire, Sheet, Strip, Bar |
Manganeso | 0.15 % Show Material materials with Manganeso of 0.15 % | T4 | EN 573-3, EN 1301, EN 1386, EN 1715-3, EN 485, EN 754, EN 755 | Profile, Rod, Flat, Plate, Tube, Wire, Sheet, Strip, Bar |
Silicona | 0.4 - 0.8 % Show Material materials with Silicona of 0.4 - 0.8 % | T4 | EN 573-3, EN 1301, EN 1386, EN 1715-3, EN 485, EN 754, EN 755 | Profile, Rod, Flat, Plate, Tube, Wire, Sheet, Strip, Bar |
Titanio | 0.15 % Show Material materials with Titanio of 0.15 % | T4 | EN 573-3, EN 1301, EN 1386, EN 1715-3, EN 485, EN 754, EN 755 | Profile, Rod, Flat, Plate, Tube, Wire, Sheet, Strip, Bar |
Zinc | 0.25 % Show Material materials with Zinc of 0.25 % | T4 | EN 573-3, EN 1301, EN 1386, EN 1715-3, EN 485, EN 754, EN 755 | Profile, Rod, Flat, Plate, Tube, Wire, Sheet, Strip, Bar |
Technological properties
Property | ||
---|---|---|
Anodizing | decorative: acceptable, Protective: very good | |
Brazing | hard brazing (with flux/ without flux): good / sufficient, friction soldering: good, soft brazing with flux: acceptable | |
Corrosion properties | Seawater: good to acceptable, weathering: good | |
Workability | Bending / Spinning (cold): acceptable (T3, T4) / good (O), Impact extrusion (cold): good (O), Deep drawing / upsetting (Condition) good (O) / good (O) |