General
Property | Temperature | Value | Condition | Related Standards |
---|---|---|---|---|
Densidad | 2.75 g/cm³ Show Material materials with Densidad of 2.75 g/cm³ | T4 | EN 1706 | |
20.0 °C | 2.75 g/cm³ Show Material materials with Densidad of 2.75 g/cm³ | T4 | DIN 1725-2, EN 1676, EN 1706, WL 3.1854 |
Mecánica
Property | Temperature | Value | Condition | Related Standards | Comment |
---|---|---|---|---|---|
Bending Fatigue Strength | 80.0 - 110.0 MPa Show Material materials with Bending Fatigue Strength of 80.0 - 110.0 MPa | T4 | EN 1706 | ||
Coeficiente de Poisson | 0.33 [-] Show Material materials with Coeficiente de Poisson of 0.33 [-] | Typical for Cast 2xx.x Series Aluminium | |||
Dureza Brinell | 90.0 [-] Show Material materials with Dureza Brinell of 90.0 [-] | T4 | EN 1706 | ||
20.0 °C | 85.0 [-] Show Material materials with Dureza Brinell of 85.0 [-] | T4 | DIN 1725-2, EN 1676, EN 1706, WL 3.1854 | ||
20.0 °C | 90.0 - 120.0 [-] Show Material materials with Dureza Brinell of 90.0 - 120.0 [-] | T4 | DIN 1725-2, EN 1676, EN 1706, WL 3.1854 | ||
20.0 °C | 90.0 [-] Show Material materials with Dureza Brinell of 90.0 [-] | T4 | DIN 1725-2, EN 1676, EN 1706, WL 3.1854 | ||
20.0 °C | 90.0 - 115.0 [-] Show Material materials with Dureza Brinell of 90.0 - 115.0 [-] | T4 | DIN 1725-2, EN 1676, EN 1706, WL 3.1854 | ||
20.0 °C | 95.0 - 115.0 [-] Show Material materials with Dureza Brinell of 95.0 - 115.0 [-] | T4 | DIN 1725-2, EN 1676, EN 1706, WL 3.1854 | ||
Elongación | 5.0 % Show Material materials with Elongación of 5.0 % | T4 | EN 1706 | A50 | |
8.0 % Show Material materials with Elongación of 8.0 % | T4 | EN 1706 | A50 | ||
20.0 °C | 3.0 % Show Material materials with Elongación of 3.0 % | T4 | DIN 1725-2, EN 1676, EN 1706, WL 3.1854 | ||
20.0 °C | 4.0 % Show Material materials with Elongación of 4.0 % | T4 | WL 3.1854, DIN 1725-2 | ||
20.0 °C | 5.0 - 10.0 % Show Material materials with Elongación of 5.0 - 10.0 % | T4 | DIN 1725-2, EN 1676, EN 1706, WL 3.1854 | ||
20.0 °C | 5.0 % Show Material materials with Elongación of 5.0 % | T4 | DIN 1725-2, EN 1676, EN 1706, WL 3.1854 | ||
20.0 °C | 5.0 - 15.0 % Show Material materials with Elongación of 5.0 - 15.0 % | T4 | DIN 1725-2, EN 1676, EN 1706, WL 3.1854 | ||
20.0 °C | 6.0 % Show Material materials with Elongación of 6.0 % | T4 | WL 3.1854, DIN 1725-2 | ||
20.0 °C | 8.0 - 18.0 % Show Material materials with Elongación of 8.0 - 18.0 % | T4 | DIN 1725-2, EN 1676, EN 1706, WL 3.1854 | ||
Módulo elástico | 72.0 GPa Show Material materials with Módulo elástico of 72.0 GPa | T4 | EN 1706 | ||
20.0 °C | 70.6 GPa Show Material materials with Módulo elástico of 70.6 GPa | T4 | WL 3.1854, DIN 1725-2 | ||
20.0 °C | 72.0 GPa Show Material materials with Módulo elástico of 72.0 GPa | T4 | DIN 1725-2, EN 1676, EN 1706, WL 3.1854 | ||
Resistencia a la tracción | 300.0 MPa Show Material materials with Resistencia a la tracción of 300.0 MPa | T4 | EN 1706 | ||
320.0 MPa Show Material materials with Resistencia a la tracción of 320.0 MPa | T4 | EN 1706 | |||
20.0 °C | 240.0 MPa Show Material materials with Resistencia a la tracción of 240.0 MPa | T4 | DIN 1725-2, EN 1676, EN 1706, WL 3.1854 | ||
20.0 °C | 270.0 MPa Show Material materials with Resistencia a la tracción of 270.0 MPa | T4 | DIN 1725-2, EN 1676, EN 1706, WL 3.1854 | ||
20.0 °C | 300.0 - 400.0 MPa Show Material materials with Resistencia a la tracción of 300.0 - 400.0 MPa | T4 | DIN 1725-2, EN 1676, EN 1706, WL 3.1854 | ||
20.0 °C | 300.0 MPa Show Material materials with Resistencia a la tracción of 300.0 MPa | T4 | WL 3.1854, DIN 1725-2 | ||
20.0 °C | 320.0 MPa Show Material materials with Resistencia a la tracción of 320.0 MPa | T4 | DIN 1725-2, EN 1676, EN 1706, WL 3.1854 | ||
20.0 °C | 320.0 - 420.0 MPa Show Material materials with Resistencia a la tracción of 320.0 - 420.0 MPa | T4 | DIN 1725-2, EN 1676, EN 1706, WL 3.1854 |
Aplicaciones térmicas
Property | Temperature | Value | Condition | Related Standards |
---|---|---|---|---|
Calor específico | 910.0 J/(kg·K) Show Material materials with Calor específico of 910.0 J/(kg·K) | T4 | EN 1706 | |
20.0 °C | 910.0 J/(kg·K) Show Material materials with Calor específico of 910.0 J/(kg·K) | T4 | DIN 1725-2, EN 1676, EN 1706, WL 3.1854 | |
Coeficiente de dilatación térmica | 20 °C | 2.3e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.3e-05 1/K | T4 | EN 1706 |
100 °C | 2.3e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.3e-05 1/K | T4 | EN 1706 | |
200.0 °C | 2.4e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.4e-05 1/K | T4 | DIN 1725-2, EN 1676, EN 1706, WL 3.1854 | |
Conductividad térmica | 120.0 - 150.0 W/(m·K) Show Material materials with Conductividad térmica of 120.0 - 150.0 W/(m·K) | T4 | EN 1706 | |
20.0 °C | 110.0 - 140.0 W/(m·K) Show Material materials with Conductividad térmica of 110.0 - 140.0 W/(m·K) | T4 | DIN 1725-2, EN 1676, EN 1706, WL 3.1854 | |
20.0 °C | 126.0 - 147.0 W/(m·K) Show Material materials with Conductividad térmica of 126.0 - 147.0 W/(m·K) | T4 | WL 3.1854, DIN 1725-2 | |
Temperatura de fusión | 540.0 - 640.0 °C Show Material materials with Temperatura de fusión of 540.0 - 640.0 °C | T4 | EN 1706 |
Eléctrico
Property | Temperature | Value | Condition | Related Standards |
---|---|---|---|---|
Conductividad eléctrica | 16000000.0 - 23000000.0 S/m Show Material materials with Conductividad eléctrica of 16000000.0 - 23000000.0 S/m | T4 | EN 1706 | |
20.0 °C | 16000000.0 - 20000000.0 S/m Show Material materials with Conductividad eléctrica of 16000000.0 - 20000000.0 S/m | T4 | DIN 1725-2, EN 1676, EN 1706, WL 3.1854 | |
20.0 °C | 17000000.0 - 19000000.0 S/m Show Material materials with Conductividad eléctrica of 17000000.0 - 19000000.0 S/m | T4 | WL 3.1854, DIN 1725-2 | |
Resistividad eléctrica | 4.35e-08 - 6.25e-08 Ω·m Show Material materials with Resistividad eléctrica of 4.35e-08 - 6.25e-08 Ω·m | T4 | EN 1706 |
Chemical properties
Property | Value | Condition | Related Standards |
---|---|---|---|
Aluminio | 93.4 % Show Material materials with Aluminio of 93.4 % | T4 | WL 3.1854, DIN 1725-2 |
93.5 % Show Material materials with Aluminio of 93.5 % | T4 | DIN 1725-2, EN 1676, EN 1706, WL 3.1854 | |
Cobre | 4.2 - 4.9 % Show Material materials with Cobre of 4.2 - 4.9 % | T4 | DIN 1725-2, EN 1676, EN 1706, WL 3.1854 |
4.2 - 5.0 % Show Material materials with Cobre of 4.2 - 5.0 % | T4 | WL 3.1854, DIN 1725-2 | |
Hierro | 0.18 % Show Material materials with Hierro of 0.18 % | T4 | DIN 1725-2, EN 1676, EN 1706, WL 3.1854 |
0.18 % Show Material materials with Hierro of 0.18 % | T4 | EN 1706 | |
0.35 % Show Material materials with Hierro of 0.35 % | T4 | WL 3.1854, DIN 1725-2 | |
Magnesio | 0.15 - 0.3 % Show Material materials with Magnesio of 0.15 - 0.3 % | T4 | DIN 1725-2, EN 1676, EN 1706, WL 3.1854 |
0.15 - 0.35 % Show Material materials with Magnesio of 0.15 - 0.35 % | T4 | WL 3.1854, DIN 1725-2 | |
Manganeso | 0.001 - 0.5 % Show Material materials with Manganeso of 0.001 - 0.5 % | T4 | DIN 1725-2, EN 1676, EN 1706, WL 3.1854 |
0.1 % Show Material materials with Manganeso of 0.1 % | T4 | WL 3.1854, DIN 1725-2 | |
Níquel | 0.03 Show Material materials with Níquel of 0.03 | T4 | WL 3.1854, DIN 1725-2 |
Silicona | 0.18 % Show Material materials with Silicona of 0.18 % | T4 | DIN 1725-2, EN 1676, EN 1706, WL 3.1854 |
0.3 % Show Material materials with Silicona of 0.3 % | T4 | WL 3.1854, DIN 1725-2 | |
Titanio | 0.15 - 0.3 % Show Material materials with Titanio of 0.15 - 0.3 % | T4 | DIN 1725-2, EN 1676, EN 1706, WL 3.1854 |
0.15 - 0.25 % Show Material materials with Titanio of 0.15 - 0.25 % | T4 | WL 3.1854, DIN 1725-2 | |
Zinc | 0.07 % Show Material materials with Zinc of 0.07 % | T4 | DIN 1725-2, EN 1676, EN 1706, WL 3.1854 |
0.1 % Show Material materials with Zinc of 0.1 % | T4 | WL 3.1854, DIN 1725-2 |
Technological properties
Property | ||
---|---|---|
Anodizing | decorative: acceptable | |
Corrosion properties | general: not sufficient | |
General machinability | as cast: excellent | |
Processing methods | investment casting, sample taken from casting |