General
Property | Temperature | Value |
---|---|---|
Densidad | 20.0 °C | 7.7 - 7.71 g/cm³ Show Material materials with Densidad of 7.7 - 7.71 g/cm³ |
Mecánica
Property | Temperature | Value | Comment |
---|---|---|---|
Coeficiente de Poisson | 23.0 °C | 0.29 [-] Show Material materials with Coeficiente de Poisson of 0.29 [-] | Typical for Chromium Steel |
Módulo elástico | 20.0 °C | 222 GPa Show Material materials with Módulo elástico of 222 GPa | |
100.0 °C | 216 GPa Show Material materials with Módulo elástico of 216 GPa | ||
200.0 °C | 209 GPa Show Material materials with Módulo elástico of 209 GPa | ||
300.0 °C | 201 GPa Show Material materials with Módulo elástico of 201 GPa | ||
400.0 °C | 192 GPa Show Material materials with Módulo elástico of 192 GPa | ||
500.0 °C | 183 GPa Show Material materials with Módulo elástico of 183 GPa | ||
600.0 °C | 174 GPa Show Material materials with Módulo elástico of 174 GPa | ||
Aplicaciones térmicas
Property | Temperature | Value | Comment |
---|---|---|---|
Calor específico | 20.0 °C | 439 J/(kg·K) Show Material materials with Calor específico of 439 J/(kg·K) | |
100.0 °C | 474 J/(kg·K) Show Material materials with Calor específico of 474 J/(kg·K) | ||
200.0 °C | 498 J/(kg·K) Show Material materials with Calor específico of 498 J/(kg·K) | ||
300.0 °C | 517 J/(kg·K) Show Material materials with Calor específico of 517 J/(kg·K) | ||
400.0 °C | 538 J/(kg·K) Show Material materials with Calor específico of 538 J/(kg·K) | ||
500.0 °C | 564 J/(kg·K) Show Material materials with Calor específico of 564 J/(kg·K) | ||
600.0 °C | 598 J/(kg·K) Show Material materials with Calor específico of 598 J/(kg·K) | ||
Coeficiente de dilatación térmica | 20.0 °C | 1.02E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.02E-5 1/K | |
100.0 °C | 1.05E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.05E-5 1/K | ||
200.0 °C | 1.09E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.09E-5 1/K | ||
300.0 °C | 1.13E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.13E-5 1/K | ||
400.0 °C | 1.16E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.16E-5 1/K | ||
500.0 °C | 1.2E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.2E-5 1/K | ||
600.0 °C | 1.22E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.22E-5 1/K | ||
Conductividad térmica | 20.0 °C | 24.6 W/(m·K) Show Material materials with Conductividad térmica of 24.6 W/(m·K) | |
100.0 °C | 24.7 W/(m·K) Show Material materials with Conductividad térmica of 24.7 W/(m·K) | ||
200.0 °C | 25 W/(m·K) Show Material materials with Conductividad térmica of 25 W/(m·K) | ||
300.0 °C | 25.2 W/(m·K) Show Material materials with Conductividad térmica of 25.2 W/(m·K) | ||
400.0 °C | 25.5 W/(m·K) Show Material materials with Conductividad térmica of 25.5 W/(m·K) | ||
500.0 °C | 25.8 W/(m·K) Show Material materials with Conductividad térmica of 25.8 W/(m·K) | ||
600.0 °C | 26 W/(m·K) Show Material materials with Conductividad térmica of 26 W/(m·K) | ||
Difusividad térmica | 20.0 °C | 7.3 mm²/s Show Material materials with Difusividad térmica of 7.3 mm²/s | |
100.0 °C | 6.4 mm²/s Show Material materials with Difusividad térmica of 6.4 mm²/s | ||
200.0 °C | 6.1 mm²/s Show Material materials with Difusividad térmica of 6.1 mm²/s | ||
300.0 °C | 5.8 mm²/s Show Material materials with Difusividad térmica of 5.8 mm²/s | ||
400.0 °C | 5.4 mm²/s Show Material materials with Difusividad térmica of 5.4 mm²/s | ||
500.0 °C | 4.8 mm²/s Show Material materials with Difusividad térmica of 4.8 mm²/s | ||
600.0 °C | 4.1 mm²/s Show Material materials with Difusividad térmica of 4.1 mm²/s | ||
Temperatura de fusión | 1382 - 1529 °C Show Material materials with Temperatura de fusión of 1382 - 1529 °C | Typical for Chromium Steel |
Eléctrico
Property | Temperature | Value |
---|---|---|
Resistividad eléctrica | 20.0 °C | 5.87E-7 Ω·m Show Material materials with Resistividad eléctrica of 5.87E-7 Ω·m |
100.0 °C | 6.55E-7 Ω·m Show Material materials with Resistividad eléctrica of 6.55E-7 Ω·m | |
200.0 °C | 7.38E-7 Ω·m Show Material materials with Resistividad eléctrica of 7.38E-7 Ω·m | |
300.0 °C | 8.19E-7 Ω·m Show Material materials with Resistividad eléctrica of 8.19E-7 Ω·m | |
400.0 °C | 8.96E-7 Ω·m Show Material materials with Resistividad eléctrica of 8.96E-7 Ω·m | |
500.0 °C | 9.7E-7 Ω·m Show Material materials with Resistividad eléctrica of 9.7E-7 Ω·m | |
600.0 °C | 1.04E-6 Ω·m Show Material materials with Resistividad eléctrica of 1.04E-6 Ω·m | |
Chemical properties
Property | Value |
---|---|
Azufre | 0.03 % Show Material materials with Azufre of 0.03 % |
Carbono | 0.42 - 0.5 % Show Material materials with Carbono of 0.42 - 0.5 % |
Cobre | 0.3 % Show Material materials with Cobre of 0.3 % |
Cromo | 12.5 - 14.5 % Show Material materials with Cromo of 12.5 - 14.5 % |
Fósforo | 0.04 % Show Material materials with Fósforo of 0.04 % |
Manganeso | 1 % Show Material materials with Manganeso of 1 % |
Níquel | 1 % Show Material materials with Níquel of 1 % |
Silicona | 1 % Show Material materials with Silicona of 1 % |