General
Property | Temperature | Value |
---|---|---|
Densidad | 20.0 °C | 7.84 g/cm³ Show Material materials with Densidad of 7.84 g/cm³ |
Mecánica
Property | Temperature | Value |
---|---|---|
Coeficiente de Poisson | 20.0 °C | 0.28 [-] Show Material materials with Coeficiente de Poisson of 0.28 [-] |
100.0 °C | 0.29 [-] Show Material materials with Coeficiente de Poisson of 0.29 [-] | |
200.0 °C | 0.3 [-] Show Material materials with Coeficiente de Poisson of 0.3 [-] | |
300.0 °C | 0.3 [-] Show Material materials with Coeficiente de Poisson of 0.3 [-] | |
400.0 °C | 0.3 [-] Show Material materials with Coeficiente de Poisson of 0.3 [-] | |
500.0 °C | 0.31 [-] Show Material materials with Coeficiente de Poisson of 0.31 [-] | |
Módulo de cizallamiento | 20.0 °C | 80.8 GPa Show Material materials with Módulo de cizallamiento of 80.8 GPa |
100.0 °C | 78.79 GPa Show Material materials with Módulo de cizallamiento of 78.79 GPa | |
200.0 °C | 75.86 GPa Show Material materials with Módulo de cizallamiento of 75.86 GPa | |
300.0 °C | 72.77 GPa Show Material materials with Módulo de cizallamiento of 72.77 GPa | |
400.0 °C | 69.37 GPa Show Material materials with Módulo de cizallamiento of 69.37 GPa | |
500.0 °C | 65.35 GPa Show Material materials with Módulo de cizallamiento of 65.35 GPa | |
Módulo elástico | -100.0 °C | 217 GPa Show Material materials with Módulo elástico of 217 GPa |
20.0 °C | 207.18 - 212 GPa Show Material materials with Módulo elástico of 207.18 - 212 GPa | |
100.0 °C | 203.16 - 207 GPa Show Material materials with Módulo elástico of 203.16 - 207 GPa | |
200.0 °C | 196.52 - 199 GPa Show Material materials with Módulo elástico of 196.52 - 199 GPa | |
300.0 °C | 188.95 - 192 GPa Show Material materials with Módulo elástico of 188.95 - 192 GPa | |
400.0 °C | 180.61 - 184 GPa Show Material materials with Módulo elástico of 180.61 - 184 GPa | |
500.0 °C | 170.87 - 175 GPa Show Material materials with Módulo elástico of 170.87 - 175 GPa | |
600.0 °C | 164 GPa Show Material materials with Módulo elástico of 164 GPa | |
Aplicaciones térmicas
Property | Temperature | Value | Comment |
---|---|---|---|
Calor específico | -100.0 °C | 423 J/(kg·K) Show Material materials with Calor específico of 423 J/(kg·K) | |
20.0 °C | 461 J/(kg·K) Show Material materials with Calor específico of 461 J/(kg·K) | ||
100.0 °C | 479 J/(kg·K) Show Material materials with Calor específico of 479 J/(kg·K) | ||
200.0 °C | 499 J/(kg·K) Show Material materials with Calor específico of 499 J/(kg·K) | ||
300.0 °C | 517 J/(kg·K) Show Material materials with Calor específico of 517 J/(kg·K) | ||
400.0 °C | 536 J/(kg·K) Show Material materials with Calor específico of 536 J/(kg·K) | ||
500.0 °C | 558 J/(kg·K) Show Material materials with Calor específico of 558 J/(kg·K) | ||
600.0 °C | 587 J/(kg·K) Show Material materials with Calor específico of 587 J/(kg·K) | ||
Coeficiente de dilatación térmica | -100.0 °C | 1.05E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.05E-5 1/K | |
20.0 °C | 1.15E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.15E-5 1/K | ||
100.0 °C | 1.21E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.21E-5 1/K | ||
200.0 °C | 1.27E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.27E-5 1/K | ||
300.0 °C | 1.32E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.32E-5 1/K | ||
400.0 °C | 1.36E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.36E-5 1/K | ||
500.0 °C | 1.4E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.4E-5 1/K | ||
600.0 °C | 1.44E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.44E-5 1/K | ||
Conductividad térmica | -100.0 °C | 31.9 W/(m·K) Show Material materials with Conductividad térmica of 31.9 W/(m·K) | |
20.0 °C | 37.6 W/(m·K) Show Material materials with Conductividad térmica of 37.6 W/(m·K) | ||
100.0 °C | 39.3 W/(m·K) Show Material materials with Conductividad térmica of 39.3 W/(m·K) | ||
200.0 °C | 40.1 W/(m·K) Show Material materials with Conductividad térmica of 40.1 W/(m·K) | ||
300.0 °C | 39.6 W/(m·K) Show Material materials with Conductividad térmica of 39.6 W/(m·K) | ||
400.0 °C | 38.4 W/(m·K) Show Material materials with Conductividad térmica of 38.4 W/(m·K) | ||
500.0 °C | 36.7 W/(m·K) Show Material materials with Conductividad térmica of 36.7 W/(m·K) | ||
600.0 °C | 34.8 W/(m·K) Show Material materials with Conductividad térmica of 34.8 W/(m·K) | ||
Difusividad térmica | -100.0 °C | 10.9 mm²/s Show Material materials with Difusividad térmica of 10.9 mm²/s | |
20.0 °C | 10.4 mm²/s Show Material materials with Difusividad térmica of 10.4 mm²/s | ||
100.0 °C | 10.1 mm²/s Show Material materials with Difusividad térmica of 10.1 mm²/s | ||
200.0 °C | 9.7 mm²/s Show Material materials with Difusividad térmica of 9.7 mm²/s | ||
300.0 °C | 9 mm²/s Show Material materials with Difusividad térmica of 9 mm²/s | ||
400.0 °C | 8.1 mm²/s Show Material materials with Difusividad térmica of 8.1 mm²/s | ||
500.0 °C | 7.1 mm²/s Show Material materials with Difusividad térmica of 7.1 mm²/s | ||
600.0 °C | 5.9 mm²/s Show Material materials with Difusividad térmica of 5.9 mm²/s | ||
Temperatura de fusión | 1370 - 1425 °C Show Material materials with Temperatura de fusión of 1370 - 1425 °C | Typical for Tool And Machining Steel |
Eléctrico
Property | Temperature | Value |
---|---|---|
Resistividad eléctrica | -100.0 °C | 2.14E-7 Ω·m Show Material materials with Resistividad eléctrica of 2.14E-7 Ω·m |
20.0 °C | 2.77E-7 Ω·m Show Material materials with Resistividad eléctrica of 2.77E-7 Ω·m | |
100.0 °C | 3.26E-7 Ω·m Show Material materials with Resistividad eléctrica of 3.26E-7 Ω·m | |
200.0 °C | 3.94E-7 Ω·m Show Material materials with Resistividad eléctrica of 3.94E-7 Ω·m | |
300.0 °C | 4.74E-7 Ω·m Show Material materials with Resistividad eléctrica of 4.74E-7 Ω·m | |
400.0 °C | 5.66E-7 Ω·m Show Material materials with Resistividad eléctrica of 5.66E-7 Ω·m | |
500.0 °C | 6.73E-7 Ω·m Show Material materials with Resistividad eléctrica of 6.73E-7 Ω·m | |
600.0 °C | 7.96E-7 Ω·m Show Material materials with Resistividad eléctrica of 7.96E-7 Ω·m | |
Chemical properties
Property | Value |
---|---|
Azufre | 0.03 % Show Material materials with Azufre of 0.03 % |
Carbono | 0.5 - 0.6 % Show Material materials with Carbono of 0.5 - 0.6 % |
Cromo | 0.6 - 0.8 % Show Material materials with Cromo of 0.6 - 0.8 % |
Fósforo | 0.03 % Show Material materials with Fósforo of 0.03 % |
Manganeso | 0.65 - 0.95 % Show Material materials with Manganeso of 0.65 - 0.95 % |
Molibdeno | 0.25 - 0.35 % Show Material materials with Molibdeno of 0.25 - 0.35 % |
Níquel | 1.5 - 1.8 % Show Material materials with Níquel of 1.5 - 1.8 % |
Silicona | 0.1 - 0.4 % Show Material materials with Silicona of 0.1 - 0.4 % |
Vanadio | 0.07 - 0.12 % Show Material materials with Vanadio of 0.07 - 0.12 % |