General
Property | Temperature | Value |
---|---|---|
Densidad | 20.0 °C | 7.9 - 7.92 g/cm³ Show Material materials with Densidad of 7.9 - 7.92 g/cm³ |
Mecánica
Property | Temperature | Value |
---|---|---|
Coeficiente de Poisson | 20.0 °C | 0.28 [-] Show Material materials with Coeficiente de Poisson of 0.28 [-] |
24.0 °C | 0.24 - 0.25 [-] Show Material materials with Coeficiente de Poisson of 0.24 - 0.25 [-] | |
149.0 °C | 0.27 - 0.3 [-] Show Material materials with Coeficiente de Poisson of 0.27 - 0.3 [-] | |
260.0 °C | 0.29 - 0.32 [-] Show Material materials with Coeficiente de Poisson of 0.29 - 0.32 [-] | |
371.0 °C | 0.32 [-] Show Material materials with Coeficiente de Poisson of 0.32 [-] | |
483.0 °C | 0.27 - 0.29 [-] Show Material materials with Coeficiente de Poisson of 0.27 - 0.29 [-] | |
593.0 °C | 0.29 - 0.3 [-] Show Material materials with Coeficiente de Poisson of 0.29 - 0.3 [-] | |
704.0 °C | 0.27 - 0.3 [-] Show Material materials with Coeficiente de Poisson of 0.27 - 0.3 [-] | |
816.0 °C | 0.23 - 0.27 [-] Show Material materials with Coeficiente de Poisson of 0.23 - 0.27 [-] | |
Elongación | 20.0 °C | 35 - 45 % Show Material materials with Elongación of 35 - 45 % |
Elongación A80 | 20.0 °C | 35 % Show Material materials with Elongación A80 of 35 % |
Elongación A80 transversal | 20.0 °C | 40 % Show Material materials with Elongación A80 transversal of 40 % |
Elongación transversal | 20.0 °C | 35 - 40 % Show Material materials with Elongación transversal of 35 - 40 % |
Límite elástico Rp 0,2 | 20.0 °C | 195 MPa Show Material materials with Límite elástico Rp 0,2 of 195 MPa |
50.0 °C | 177 MPa Show Material materials with Límite elástico Rp 0,2 of 177 MPa | |
100.0 °C | 157 MPa Show Material materials with Límite elástico Rp 0,2 of 157 MPa | |
150.0 °C | 142 MPa Show Material materials with Límite elástico Rp 0,2 of 142 MPa | |
200.0 °C | 127 MPa Show Material materials with Límite elástico Rp 0,2 of 127 MPa | |
250.0 °C | 118 MPa Show Material materials with Límite elástico Rp 0,2 of 118 MPa | |
300.0 °C | 110 MPa Show Material materials with Límite elástico Rp 0,2 of 110 MPa | |
350.0 °C | 104 MPa Show Material materials with Límite elástico Rp 0,2 of 104 MPa | |
400.0 °C | 98 MPa Show Material materials with Límite elástico Rp 0,2 of 98 MPa | |
450.0 °C | 95 MPa Show Material materials with Límite elástico Rp 0,2 of 95 MPa | |
500.0 °C | 92 MPa Show Material materials with Límite elástico Rp 0,2 of 92 MPa | |
550.0 °C | 90 MPa Show Material materials with Límite elástico Rp 0,2 of 90 MPa | |
Límite elástico Rp 1,0 | 20.0 °C | 230 MPa Show Material materials with Límite elástico Rp 1,0 of 230 MPa |
50.0 °C | 211 MPa Show Material materials with Límite elástico Rp 1,0 of 211 MPa | |
100.0 °C | 191 MPa Show Material materials with Límite elástico Rp 1,0 of 191 MPa | |
150.0 °C | 172 MPa Show Material materials with Límite elástico Rp 1,0 of 172 MPa | |
200.0 °C | 157 MPa Show Material materials with Límite elástico Rp 1,0 of 157 MPa | |
250.0 °C | 145 MPa Show Material materials with Límite elástico Rp 1,0 of 145 MPa | |
300.0 °C | 135 MPa Show Material materials with Límite elástico Rp 1,0 of 135 MPa | |
350.0 °C | 129 MPa Show Material materials with Límite elástico Rp 1,0 of 129 MPa | |
400.0 °C | 125 MPa Show Material materials with Límite elástico Rp 1,0 of 125 MPa | |
450.0 °C | 122 MPa Show Material materials with Límite elástico Rp 1,0 of 122 MPa | |
500.0 °C | 120 MPa Show Material materials with Límite elástico Rp 1,0 of 120 MPa | |
550.0 °C | 120 MPa Show Material materials with Límite elástico Rp 1,0 of 120 MPa | |
Límite elástico transversal Rp 0,2 | 20.0 °C | 195 MPa Show Material materials with Límite elástico transversal Rp 0,2 of 195 MPa |
Límite elástico transversal Rp 1,0 | 20.0 °C | 230 MPa Show Material materials with Límite elástico transversal Rp 1,0 of 230 MPa |
Módulo de cizallamiento | 24.0 °C | 78.6 GPa Show Material materials with Módulo de cizallamiento of 78.6 GPa |
149.0 °C | 72.4 - 74.5 GPa Show Material materials with Módulo de cizallamiento of 72.4 - 74.5 GPa | |
260.0 °C | 69.6 - 71 GPa Show Material materials with Módulo de cizallamiento of 69.6 - 71 GPa | |
371.0 °C | 65.5 - 67.6 GPa Show Material materials with Módulo de cizallamiento of 65.5 - 67.6 GPa | |
483.0 °C | 62.1 GPa Show Material materials with Módulo de cizallamiento of 62.1 GPa | |
593.0 °C | 57.9 - 60 GPa Show Material materials with Módulo de cizallamiento of 57.9 - 60 GPa | |
704.0 °C | 54.5 - 55.9 GPa Show Material materials with Módulo de cizallamiento of 54.5 - 55.9 GPa | |
816.0 °C | 49 - 50.3 GPa Show Material materials with Módulo de cizallamiento of 49 - 50.3 GPa | |
Módulo elástico | -100.0 °C | 206 GPa Show Material materials with Módulo elástico of 206 GPa |
20.0 °C | 196 - 200 GPa Show Material materials with Módulo elástico of 196 - 200 GPa | |
24.0 °C | 194.4 - 196.5 GPa Show Material materials with Módulo elástico of 194.4 - 196.5 GPa | |
100.0 °C | 190 - 194 GPa Show Material materials with Módulo elástico of 190 - 194 GPa | |
149.0 °C | 188.2 - 189.6 GPa Show Material materials with Módulo elástico of 188.2 - 189.6 GPa | |
200.0 °C | 182 - 186 GPa Show Material materials with Módulo elástico of 182 - 186 GPa | |
260.0 °C | 182.7 - 184.1 GPa Show Material materials with Módulo elástico of 182.7 - 184.1 GPa | |
300.0 °C | 174 - 179 GPa Show Material materials with Módulo elástico of 174 - 179 GPa | |
371.0 °C | 173.1 - 177.9 GPa Show Material materials with Módulo elástico of 173.1 - 177.9 GPa | |
400.0 °C | 166 - 172 GPa Show Material materials with Módulo elástico of 166 - 172 GPa | |
483.0 °C | 157.9 - 160 GPa Show Material materials with Módulo elástico of 157.9 - 160 GPa | |
500.0 °C | 158 - 165 GPa Show Material materials with Módulo elástico of 158 - 165 GPa | |
593.0 °C | 149.6 - 155.8 GPa Show Material materials with Módulo elástico of 149.6 - 155.8 GPa | |
600.0 °C | 150 GPa Show Material materials with Módulo elástico of 150 GPa | |
700.0 °C | 142 GPa Show Material materials with Módulo elástico of 142 GPa | |
704.0 °C | 137.9 - 144.8 GPa Show Material materials with Módulo elástico of 137.9 - 144.8 GPa | |
800.0 °C | 134 GPa Show Material materials with Módulo elástico of 134 GPa | |
816.0 °C | 120.7 - 128.2 GPa Show Material materials with Módulo elástico of 120.7 - 128.2 GPa | |
Resistencia a la tracción | 20.0 °C | 500 - 700 MPa Show Material materials with Resistencia a la tracción of 500 - 700 MPa |
Resistencia a la tracción transversal | 20.0 °C | 500 - 700 MPa Show Material materials with Resistencia a la tracción transversal of 500 - 700 MPa |
Aplicaciones térmicas
Property | Temperature | Value | Comment |
---|---|---|---|
Calor específico | -100.0 °C | 440 J/(kg·K) Show Material materials with Calor específico of 440 J/(kg·K) | |
20.0 °C | 472 - 500 J/(kg·K) Show Material materials with Calor específico of 472 - 500 J/(kg·K) | ||
100.0 °C | 487 J/(kg·K) Show Material materials with Calor específico of 487 J/(kg·K) | ||
200.0 °C | 503 J/(kg·K) Show Material materials with Calor específico of 503 J/(kg·K) | ||
300.0 °C | 512 J/(kg·K) Show Material materials with Calor específico of 512 J/(kg·K) | ||
400.0 °C | 520 J/(kg·K) Show Material materials with Calor específico of 520 J/(kg·K) | ||
500.0 °C | 530 J/(kg·K) Show Material materials with Calor específico of 530 J/(kg·K) | ||
600.0 °C | 541 J/(kg·K) Show Material materials with Calor específico of 541 J/(kg·K) | ||
700.0 °C | 551 J/(kg·K) Show Material materials with Calor específico of 551 J/(kg·K) | ||
800.0 °C | 559 J/(kg·K) Show Material materials with Calor específico of 559 J/(kg·K) | ||
Coeficiente de dilatación térmica | -100.0 °C | 1.49E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.49E-5 1/K | |
20.0 °C | 1.61E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.61E-5 1/K | ||
100.0 °C | 1.6E-5 - 1.67E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.6E-5 - 1.67E-5 1/K | ||
200.0 °C | 1.7E-5 - 1.72E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.7E-5 - 1.72E-5 1/K | ||
300.0 °C | 1.7E-5 - 1.77E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.7E-5 - 1.77E-5 1/K | ||
400.0 °C | 1.8E-5 - 1.81E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.8E-5 - 1.81E-5 1/K | ||
500.0 °C | 1.8E-5 - 1.84E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.8E-5 - 1.84E-5 1/K | ||
600.0 °C | 1.88E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.88E-5 1/K | ||
700.0 °C | 1.91E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.91E-5 1/K | ||
800.0 °C | 1.94E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.94E-5 1/K | ||
Conductividad térmica | -100.0 °C | 11.7 W/(m·K) Show Material materials with Conductividad térmica of 11.7 W/(m·K) | |
20.0 °C | 14.5 - 15 W/(m·K) Show Material materials with Conductividad térmica of 14.5 - 15 W/(m·K) | ||
100.0 °C | 16 W/(m·K) Show Material materials with Conductividad térmica of 16 W/(m·K) | ||
200.0 °C | 17.6 W/(m·K) Show Material materials with Conductividad térmica of 17.6 W/(m·K) | ||
300.0 °C | 19.1 W/(m·K) Show Material materials with Conductividad térmica of 19.1 W/(m·K) | ||
400.0 °C | 20.4 W/(m·K) Show Material materials with Conductividad térmica of 20.4 W/(m·K) | ||
500.0 °C | 21.9 W/(m·K) Show Material materials with Conductividad térmica of 21.9 W/(m·K) | ||
600.0 °C | 23.3 W/(m·K) Show Material materials with Conductividad térmica of 23.3 W/(m·K) | ||
700.0 °C | 24.7 W/(m·K) Show Material materials with Conductividad térmica of 24.7 W/(m·K) | ||
800.0 °C | 26.1 W/(m·K) Show Material materials with Conductividad térmica of 26.1 W/(m·K) | ||
Difusividad térmica | -100.0 °C | 3.7 mm²/s Show Material materials with Difusividad térmica of 3.7 mm²/s | |
20.0 °C | 3.9 mm²/s Show Material materials with Difusividad térmica of 3.9 mm²/s | ||
100.0 °C | 4.3 mm²/s Show Material materials with Difusividad térmica of 4.3 mm²/s | ||
200.0 °C | 4.3 mm²/s Show Material materials with Difusividad térmica of 4.3 mm²/s | ||
300.0 °C | 4.6 mm²/s Show Material materials with Difusividad térmica of 4.6 mm²/s | ||
400.0 °C | 4.7 mm²/s Show Material materials with Difusividad térmica of 4.7 mm²/s | ||
500.0 °C | 4.9 mm²/s Show Material materials with Difusividad térmica of 4.9 mm²/s | ||
600.0 °C | 5 mm²/s Show Material materials with Difusividad térmica of 5 mm²/s | ||
700.0 °C | 5.3 mm²/s Show Material materials with Difusividad térmica of 5.3 mm²/s | ||
800.0 °C | 5.7 mm²/s Show Material materials with Difusividad térmica of 5.7 mm²/s | ||
Temperatura de fusión | 1230 - 1480 °C Show Material materials with Temperatura de fusión of 1230 - 1480 °C | Typical for Austenitic Stainless Steel | |
Temperatura máx. de funcionamiento, largo | -200 - 550 °C Show Material materials with Temperatura máx. de funcionamiento, largo of -200 - 550 °C |
Eléctrico
Property | Temperature | Value |
---|---|---|
Resistividad eléctrica | -100.0 °C | 5.86E-7 Ω·m Show Material materials with Resistividad eléctrica of 5.86E-7 Ω·m |
20.0 °C | 6.92E-7 - 7.3E-7 Ω·m Show Material materials with Resistividad eléctrica of 6.92E-7 - 7.3E-7 Ω·m | |
100.0 °C | 7.58E-7 Ω·m Show Material materials with Resistividad eléctrica of 7.58E-7 Ω·m | |
200.0 °C | 8.36E-7 Ω·m Show Material materials with Resistividad eléctrica of 8.36E-7 Ω·m | |
300.0 °C | 9.07E-7 Ω·m Show Material materials with Resistividad eléctrica of 9.07E-7 Ω·m | |
400.0 °C | 9.73E-7 Ω·m Show Material materials with Resistividad eléctrica of 9.73E-7 Ω·m | |
500.0 °C | 1.02E-6 Ω·m Show Material materials with Resistividad eléctrica of 1.02E-6 Ω·m | |
600.0 °C | 1.06E-6 Ω·m Show Material materials with Resistividad eléctrica of 1.06E-6 Ω·m | |
700.0 °C | 1.1E-6 Ω·m Show Material materials with Resistividad eléctrica of 1.1E-6 Ω·m | |
800.0 °C | 1.13E-6 Ω·m Show Material materials with Resistividad eléctrica of 1.13E-6 Ω·m | |
Chemical properties
Property | Value |
---|---|
Azufre | 0.015 - 0.03 % Show Material materials with Azufre of 0.015 - 0.03 % |
Carbono | 0.07 % Show Material materials with Carbono of 0.07 % |
Cromo | 17 - 19.5 % Show Material materials with Cromo of 17 - 19.5 % |
Fósforo | 0.05 % Show Material materials with Fósforo of 0.05 % |
Manganeso | 2 % Show Material materials with Manganeso of 2 % |
Nitrógeno | 0.11 % Show Material materials with Nitrógeno of 0.11 % |
Níquel | 8 - 10.5 % Show Material materials with Níquel of 8 - 10.5 % |
Silicona | 1 % Show Material materials with Silicona of 1 % |