General
Property | Temperature | Value |
---|---|---|
Densidad | 20.0 °C | 7.58 - 7.7 g/cm³ Show Material materials with Densidad of 7.58 - 7.7 g/cm³ |
Mecánica
Property | Temperature | Value | Comment |
---|---|---|---|
Coeficiente de Poisson | 23.0 °C | 0.3 [-] Show Material materials with Coeficiente de Poisson of 0.3 [-] | Typical for Ferritic Stainless Steel |
Dureza Brinell | 20.0 °C | 185 [-] Show Material materials with Dureza Brinell of 185 [-] | |
Dureza Vickers | 20.0 °C | 185 [-] Show Material materials with Dureza Vickers of 185 [-] | |
Elongación | 20.0 °C | 20 % Show Material materials with Elongación of 20 % | |
Elongación transversal | 20.0 °C | 15 % Show Material materials with Elongación transversal of 15 % | |
Hardness, Brinell, trans | 20.0 °C | 185 [-] Show Material materials with Hardness, Brinell, trans of 185 [-] | |
Límite elástico | 20.0 °C | 250 MPa Show Material materials with Límite elástico of 250 MPa | |
Límite elástico Rp 0,2 | 20.0 °C | 240 - 250 MPa Show Material materials with Límite elástico Rp 0,2 of 240 - 250 MPa | |
50.0 °C | 235 - 240 MPa Show Material materials with Límite elástico Rp 0,2 of 235 - 240 MPa | ||
100.0 °C | 230 - 235 MPa Show Material materials with Límite elástico Rp 0,2 of 230 - 235 MPa | ||
150.0 °C | 225 - 230 MPa Show Material materials with Límite elástico Rp 0,2 of 225 - 230 MPa | ||
200.0 °C | 225 MPa Show Material materials with Límite elástico Rp 0,2 of 225 MPa | ||
250.0 °C | 220 - 225 MPa Show Material materials with Límite elástico Rp 0,2 of 220 - 225 MPa | ||
300.0 °C | 210 - 220 MPa Show Material materials with Límite elástico Rp 0,2 of 210 - 220 MPa | ||
350.0 °C | 195 - 210 MPa Show Material materials with Límite elástico Rp 0,2 of 195 - 210 MPa | ||
400.0 °C | 195 MPa Show Material materials with Límite elástico Rp 0,2 of 195 MPa | ||
Límite elástico transversal | 20.0 °C | 250 MPa Show Material materials with Límite elástico transversal of 250 MPa | |
Límite elástico transversal Rp 0,2 | 20.0 °C | 250 MPa Show Material materials with Límite elástico transversal Rp 0,2 of 250 MPa | |
Módulo de cizallamiento | 23.0 °C | 77 GPa Show Material materials with Módulo de cizallamiento of 77 GPa | Typical for Ferritic Stainless Steel |
Módulo elástico | 20.0 °C | 216 - 220 GPa Show Material materials with Módulo elástico of 216 - 220 GPa | |
100.0 °C | 213 - 215 GPa Show Material materials with Módulo elástico of 213 - 215 GPa | ||
200.0 °C | 206 - 210 GPa Show Material materials with Módulo elástico of 206 - 210 GPa | ||
300.0 °C | 198 - 205 GPa Show Material materials with Módulo elástico of 198 - 205 GPa | ||
400.0 °C | 190 - 195 GPa Show Material materials with Módulo elástico of 190 - 195 GPa | ||
500.0 °C | 180 GPa Show Material materials with Módulo elástico of 180 GPa | ||
600.0 °C | 167 GPa Show Material materials with Módulo elástico of 167 GPa | ||
700.0 °C | 150 GPa Show Material materials with Módulo elástico of 150 GPa | ||
Resistencia a la tracción | 20.0 °C | 400 - 600 MPa Show Material materials with Resistencia a la tracción of 400 - 600 MPa | |
Resistencia a la tracción transversal | 20.0 °C | 400 - 600 MPa Show Material materials with Resistencia a la tracción transversal of 400 - 600 MPa |
Aplicaciones térmicas
Property | Temperature | Value | Comment |
---|---|---|---|
Calor específico | 20.0 °C | 439 - 460 J/(kg·K) Show Material materials with Calor específico of 439 - 460 J/(kg·K) | |
100.0 °C | 474 J/(kg·K) Show Material materials with Calor específico of 474 J/(kg·K) | ||
200.0 °C | 492 J/(kg·K) Show Material materials with Calor específico of 492 J/(kg·K) | ||
300.0 °C | 517 J/(kg·K) Show Material materials with Calor específico of 517 J/(kg·K) | ||
400.0 °C | 538 J/(kg·K) Show Material materials with Calor específico of 538 J/(kg·K) | ||
500.0 °C | 564 J/(kg·K) Show Material materials with Calor específico of 564 J/(kg·K) | ||
600.0 °C | 598 J/(kg·K) Show Material materials with Calor específico of 598 J/(kg·K) | ||
700.0 °C | 647 J/(kg·K) Show Material materials with Calor específico of 647 J/(kg·K) | ||
Coeficiente de dilatación térmica | 20.0 °C | 1.02E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.02E-5 1/K | |
100.0 °C | 1.05E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.05E-5 1/K | ||
200.0 °C | 1.09E-5 - 1.1E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.09E-5 - 1.1E-5 1/K | ||
300.0 °C | 1.13E-5 - 1.15E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.13E-5 - 1.15E-5 1/K | ||
400.0 °C | 1.16E-5 - 1.2E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.16E-5 - 1.2E-5 1/K | ||
500.0 °C | 1.2E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.2E-5 1/K | ||
600.0 °C | 1.22E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.22E-5 1/K | ||
700.0 °C | 1.24E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.24E-5 1/K | ||
Conductividad térmica | 20.0 °C | 15.7 - 30 W/(m·K) Show Material materials with Conductividad térmica of 15.7 - 30 W/(m·K) | |
100.0 °C | 17.1 W/(m·K) Show Material materials with Conductividad térmica of 17.1 W/(m·K) | ||
200.0 °C | 18.6 W/(m·K) Show Material materials with Conductividad térmica of 18.6 W/(m·K) | ||
300.0 °C | 20 W/(m·K) Show Material materials with Conductividad térmica of 20 W/(m·K) | ||
400.0 °C | 21.2 W/(m·K) Show Material materials with Conductividad térmica of 21.2 W/(m·K) | ||
500.0 °C | 22.3 W/(m·K) Show Material materials with Conductividad térmica of 22.3 W/(m·K) | ||
600.0 °C | 23.1 W/(m·K) Show Material materials with Conductividad térmica of 23.1 W/(m·K) | ||
700.0 °C | 23.8 W/(m·K) Show Material materials with Conductividad térmica of 23.8 W/(m·K) | ||
Difusividad térmica | 20.0 °C | 4.7 mm²/s Show Material materials with Difusividad térmica of 4.7 mm²/s | |
100.0 °C | 4.5 mm²/s Show Material materials with Difusividad térmica of 4.5 mm²/s | ||
200.0 °C | 4.6 mm²/s Show Material materials with Difusividad térmica of 4.6 mm²/s | ||
300.0 °C | 4.7 mm²/s Show Material materials with Difusividad térmica of 4.7 mm²/s | ||
400.0 °C | 4.5 mm²/s Show Material materials with Difusividad térmica of 4.5 mm²/s | ||
500.0 °C | 4.3 mm²/s Show Material materials with Difusividad térmica of 4.3 mm²/s | ||
600.0 °C | 3.7 mm²/s Show Material materials with Difusividad térmica of 3.7 mm²/s | ||
700.0 °C | 3 mm²/s Show Material materials with Difusividad térmica of 3 mm²/s | ||
Temperatura de fusión | 1425 - 1530 °C Show Material materials with Temperatura de fusión of 1425 - 1530 °C | Typical for Ferritic Stainless Steel | |
Temperatura máx. de funcionamiento, largo | 0 - 600 °C Show Material materials with Temperatura máx. de funcionamiento, largo of 0 - 600 °C |
Eléctrico
Property | Temperature | Value |
---|---|---|
Resistividad eléctrica | 20.0 °C | 6E-7 - 9.19E-7 Ω·m Show Material materials with Resistividad eléctrica of 6E-7 - 9.19E-7 Ω·m |
100.0 °C | 9.48E-7 Ω·m Show Material materials with Resistividad eléctrica of 9.48E-7 Ω·m | |
200.0 °C | 9.87E-7 Ω·m Show Material materials with Resistividad eléctrica of 9.87E-7 Ω·m | |
300.0 °C | 1.03E-6 Ω·m Show Material materials with Resistividad eléctrica of 1.03E-6 Ω·m | |
400.0 °C | 1.07E-6 Ω·m Show Material materials with Resistividad eléctrica of 1.07E-6 Ω·m | |
500.0 °C | 1.12E-6 Ω·m Show Material materials with Resistividad eléctrica of 1.12E-6 Ω·m | |
600.0 °C | 1.18E-6 Ω·m Show Material materials with Resistividad eléctrica of 1.18E-6 Ω·m | |
700.0 °C | 1.24E-6 Ω·m Show Material materials with Resistividad eléctrica of 1.24E-6 Ω·m | |
Chemical properties
Property | Value |
---|---|
Aluminio | 0.1 - 0.3 % Show Material materials with Aluminio of 0.1 - 0.3 % |
Azufre | 0.015 - 0.03 % Show Material materials with Azufre of 0.015 - 0.03 % |
Carbono | 0.08 % Show Material materials with Carbono of 0.08 % |
Cromo | 12 - 14 % Show Material materials with Cromo of 12 - 14 % |
Fósforo | 0.04 - 0.05 % Show Material materials with Fósforo of 0.04 - 0.05 % |
Manganeso | 1 % Show Material materials with Manganeso of 1 % |
Silicona | 1 % Show Material materials with Silicona of 1 % |