General
Property | Temperature | Value |
---|---|---|
Densidad | 20.0 °C | 7.56 - 7.7 g/cm³ Show Material materials with Densidad of 7.56 - 7.7 g/cm³ |
Mecánica
Property | Temperature | Value | Comment |
---|---|---|---|
Coeficiente de Poisson | 23.0 °C | 0.3 [-] Show Material materials with Coeficiente de Poisson of 0.3 [-] | Typical for Ferritic Stainless Steel |
Dureza Brinell | 20.0 °C | 185 [-] Show Material materials with Dureza Brinell of 185 [-] | |
Dureza Vickers | 20.0 °C | 185 [-] Show Material materials with Dureza Vickers of 185 [-] | |
Elongación | 20.0 °C | 20 - 23 % Show Material materials with Elongación of 20 - 23 % | |
Elongación A80 | 20.0 °C | 18 - 23 % Show Material materials with Elongación A80 of 18 - 23 % | |
Elongación transversal | 20.0 °C | 18 % Show Material materials with Elongación transversal of 18 % | |
Hardness, Brinell, trans | 20.0 °C | 185 [-] Show Material materials with Hardness, Brinell, trans of 185 [-] | |
Límite elástico | 20.0 °C | 270 MPa Show Material materials with Límite elástico of 270 MPa | |
Límite elástico Rp 0,2 | 20.0 °C | 230 - 270 MPa Show Material materials with Límite elástico Rp 0,2 of 230 - 270 MPa | |
100.0 °C | 195 MPa Show Material materials with Límite elástico Rp 0,2 of 195 MPa | ||
150.0 °C | 190 MPa Show Material materials with Límite elástico Rp 0,2 of 190 MPa | ||
200.0 °C | 185 MPa Show Material materials with Límite elástico Rp 0,2 of 185 MPa | ||
250.0 °C | 175 MPa Show Material materials with Límite elástico Rp 0,2 of 175 MPa | ||
300.0 °C | 165 MPa Show Material materials with Límite elástico Rp 0,2 of 165 MPa | ||
350.0 °C | 155 MPa Show Material materials with Límite elástico Rp 0,2 of 155 MPa | ||
Límite elástico transversal | 20.0 °C | 270 MPa Show Material materials with Límite elástico transversal of 270 MPa | |
Límite elástico transversal Rp 0,2 | 20.0 °C | 270 MPa Show Material materials with Límite elástico transversal Rp 0,2 of 270 MPa | |
Módulo de cizallamiento | 23.0 °C | 77 GPa Show Material materials with Módulo de cizallamiento of 77 GPa | Typical for Ferritic Stainless Steel |
Módulo elástico | 20.0 °C | 218 - 220 GPa Show Material materials with Módulo elástico of 218 - 220 GPa | |
100.0 °C | 213 - 218 GPa Show Material materials with Módulo elástico of 213 - 218 GPa | ||
200.0 °C | 206 - 212 GPa Show Material materials with Módulo elástico of 206 - 212 GPa | ||
300.0 °C | 198 - 205 GPa Show Material materials with Módulo elástico of 198 - 205 GPa | ||
400.0 °C | 190 - 197 GPa Show Material materials with Módulo elástico of 190 - 197 GPa | ||
500.0 °C | 180 GPa Show Material materials with Módulo elástico of 180 GPa | ||
600.0 °C | 167 GPa Show Material materials with Módulo elástico of 167 GPa | ||
700.0 °C | 150 GPa Show Material materials with Módulo elástico of 150 GPa | ||
Resistencia a la tracción | 20.0 °C | 420 - 600 MPa Show Material materials with Resistencia a la tracción of 420 - 600 MPa | |
Resistencia a la tracción transversal | 20.0 °C | 430 - 600 MPa Show Material materials with Resistencia a la tracción transversal of 430 - 600 MPa |
Aplicaciones térmicas
Property | Temperature | Value | Comment |
---|---|---|---|
Calor específico | 20.0 °C | 450 - 460 J/(kg·K) Show Material materials with Calor específico of 450 - 460 J/(kg·K) | |
100.0 °C | 482 J/(kg·K) Show Material materials with Calor específico of 482 J/(kg·K) | ||
200.0 °C | 506 J/(kg·K) Show Material materials with Calor específico of 506 J/(kg·K) | ||
300.0 °C | 525 J/(kg·K) Show Material materials with Calor específico of 525 J/(kg·K) | ||
400.0 °C | 547 J/(kg·K) Show Material materials with Calor específico of 547 J/(kg·K) | ||
500.0 °C | 576 J/(kg·K) Show Material materials with Calor específico of 576 J/(kg·K) | ||
600.0 °C | 616 J/(kg·K) Show Material materials with Calor específico of 616 J/(kg·K) | ||
Coeficiente de dilatación térmica | 20.0 °C | 9.9E-6 1/K Show Material materials with Coeficiente de dilatación térmica of 9.9E-6 1/K | |
100.0 °C | 1E-5 - 1.03E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1E-5 - 1.03E-5 1/K | ||
200.0 °C | 1E-5 - 1.08E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1E-5 - 1.08E-5 1/K | ||
300.0 °C | 1.05E-5 - 1.12E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.05E-5 - 1.12E-5 1/K | ||
400.0 °C | 1.05E-5 - 1.16E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.05E-5 - 1.16E-5 1/K | ||
500.0 °C | 1.1E-5 - 1.19E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.1E-5 - 1.19E-5 1/K | ||
600.0 °C | 1.21E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.21E-5 1/K | ||
700.0 °C | 1.24E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.24E-5 1/K | ||
800.0 °C | 1.29E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.29E-5 1/K | ||
Conductividad térmica | 20.0 °C | 16 - 25 W/(m·K) Show Material materials with Conductividad térmica of 16 - 25 W/(m·K) | |
100.0 °C | 17.2 W/(m·K) Show Material materials with Conductividad térmica of 17.2 W/(m·K) | ||
200.0 °C | 18.6 W/(m·K) Show Material materials with Conductividad térmica of 18.6 W/(m·K) | ||
300.0 °C | 20 W/(m·K) Show Material materials with Conductividad térmica of 20 W/(m·K) | ||
400.0 °C | 21.2 W/(m·K) Show Material materials with Conductividad térmica of 21.2 W/(m·K) | ||
500.0 °C | 22.3 W/(m·K) Show Material materials with Conductividad térmica of 22.3 W/(m·K) | ||
600.0 °C | 23.3 W/(m·K) Show Material materials with Conductividad térmica of 23.3 W/(m·K) | ||
700.0 °C | 24.1 W/(m·K) Show Material materials with Conductividad térmica of 24.1 W/(m·K) | ||
800.0 °C | 25.5 W/(m·K) Show Material materials with Conductividad térmica of 25.5 W/(m·K) | ||
900.0 °C | 26.9 W/(m·K) Show Material materials with Conductividad térmica of 26.9 W/(m·K) | ||
1000.0 °C | 28.3 W/(m·K) Show Material materials with Conductividad térmica of 28.3 W/(m·K) | ||
Difusividad térmica | 20.0 °C | 4.7 mm²/s Show Material materials with Difusividad térmica of 4.7 mm²/s | |
100.0 °C | 4.5 mm²/s Show Material materials with Difusividad térmica of 4.5 mm²/s | ||
200.0 °C | 4.5 mm²/s Show Material materials with Difusividad térmica of 4.5 mm²/s | ||
300.0 °C | 4.6 mm²/s Show Material materials with Difusividad térmica of 4.6 mm²/s | ||
400.0 °C | 4.4 mm²/s Show Material materials with Difusividad térmica of 4.4 mm²/s | ||
500.0 °C | 4.1 mm²/s Show Material materials with Difusividad térmica of 4.1 mm²/s | ||
600.0 °C | 3.6 mm²/s Show Material materials with Difusividad térmica of 3.6 mm²/s | ||
Temperatura de fusión | 1425 - 1530 °C Show Material materials with Temperatura de fusión of 1425 - 1530 °C | Typical for Ferritic Stainless Steel |
Eléctrico
Property | Temperature | Value |
---|---|---|
Resistividad eléctrica | 20.0 °C | 6E-7 - 9.06E-7 Ω·m Show Material materials with Resistividad eléctrica of 6E-7 - 9.06E-7 Ω·m |
100.0 °C | 9.42E-7 Ω·m Show Material materials with Resistividad eléctrica of 9.42E-7 Ω·m | |
200.0 °C | 9.87E-7 Ω·m Show Material materials with Resistividad eléctrica of 9.87E-7 Ω·m | |
300.0 °C | 1.03E-6 Ω·m Show Material materials with Resistividad eléctrica of 1.03E-6 Ω·m | |
400.0 °C | 1.08E-6 Ω·m Show Material materials with Resistividad eléctrica of 1.08E-6 Ω·m | |
500.0 °C | 1.12E-6 Ω·m Show Material materials with Resistividad eléctrica of 1.12E-6 Ω·m | |
600.0 °C | 1.18E-6 Ω·m Show Material materials with Resistividad eléctrica of 1.18E-6 Ω·m | |
700.0 °C | 1.22E-6 Ω·m Show Material materials with Resistividad eléctrica of 1.22E-6 Ω·m | |
800.0 °C | 1.24E-6 Ω·m Show Material materials with Resistividad eléctrica of 1.24E-6 Ω·m | |
900.0 °C | 1.26E-6 Ω·m Show Material materials with Resistividad eléctrica of 1.26E-6 Ω·m | |
1000.0 °C | 1.27E-6 Ω·m Show Material materials with Resistividad eléctrica of 1.27E-6 Ω·m | |
Chemical properties
Property | Value |
---|---|
Azufre | 0.015 - 0.03 % Show Material materials with Azufre of 0.015 - 0.03 % |
Carbono | 0.05 % Show Material materials with Carbono of 0.05 % |
Cromo | 16 - 18 % Show Material materials with Cromo of 16 - 18 % |
Fósforo | 0.04 % Show Material materials with Fósforo of 0.04 % |
Manganeso | 1 % Show Material materials with Manganeso of 1 % |
Silicona | 1 % Show Material materials with Silicona of 1 % |
Titanio | 0.8 % Show Material materials with Titanio of 0.8 % |