General
Property | Temperature | Value | Comment |
---|---|---|---|
Densidad | 23.0 °C | 7.7 - 8.7 g/cm³ Show Material materials with Densidad of 7.7 - 8.7 g/cm³ | Typical for Leaded Phosphor Bronze |
Mecánica
Property | Temperature | Value | Comment |
---|---|---|---|
Coeficiente de Poisson | 23.0 °C | 0.33 [-] Show Material materials with Coeficiente de Poisson of 0.33 [-] | Typical for Leaded Phosphor Bronze |
Límite elástico | 23.0 °C | 130 MPa Show Material materials with Límite elástico of 130 MPa | |
Módulo elástico | 23.0 °C | 110 - 130 GPa Show Material materials with Módulo elástico of 110 - 130 GPa | Typical for Leaded Phosphor Bronze |
Resistencia a la tracción | 23.0 °C | 345 MPa Show Material materials with Resistencia a la tracción of 345 MPa |
Aplicaciones térmicas
Property | Temperature | Value | Comment |
---|---|---|---|
Calor específico | 23.0 °C | 380 J/(kg·K) Show Material materials with Calor específico of 380 J/(kg·K) | Typical for Leaded Phosphor Bronze |
Coeficiente de dilatación térmica | 23.0 °C | 1.5E-5 - 1.9E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.5E-5 - 1.9E-5 1/K | Typical for Leaded Phosphor Bronze |
Chemical properties
Property | Value |
---|---|
Aluminio | 5 - 6.5 % Show Material materials with Aluminio of 5 - 6.5 % |
Arsénico | 0.02 - 0.35 % Show Material materials with Arsénico of 0.02 - 0.35 % |
Hierro | 0.1 % Show Material materials with Hierro of 0.1 % |
Plomo | 0.1 % Show Material materials with Plomo of 0.1 % |