Mecánica
Property | Temperature | Value | Comment |
---|---|---|---|
Coeficiente de Poisson | 23.0 °C | 0.34 [-] Show Material materials with Coeficiente de Poisson of 0.34 [-] | Typical for Cast Copper Nickel Grade |
Dureza Rockwell C | 23.0 °C | 32 [-] Show Material materials with Dureza Rockwell C of 32 [-] | |
Elongación A50 | 23.0 °C | 4 % Show Material materials with Elongación A50 of 4 % | |
Límite elástico Rp0.5 | 23.0 °C | 724 MPa Show Material materials with Límite elástico Rp0.5 of 724 MPa | |
Módulo elástico | 23.0 °C | 120 - 156 GPa Show Material materials with Módulo elástico of 120 - 156 GPa | Typical for Cast Copper Nickel Grade |
Resistencia a la tracción | 23.0 °C | 758 MPa Show Material materials with Resistencia a la tracción of 758 MPa |
Aplicaciones térmicas
Property | Temperature | Value | Comment |
---|---|---|---|
Calor específico | 23.0 °C | 377 J/(kg·K) Show Material materials with Calor específico of 377 J/(kg·K) | Typical for Cast Copper Nickel Grade |
Coeficiente de dilatación térmica | 23.0 °C | 1.8E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.8E-5 1/K | Typical for Cast Copper Nickel Grade |
Conductividad térmica | 23.0 °C | 23 - 45 W/(m·K) Show Material materials with Conductividad térmica of 23 - 45 W/(m·K) | Typical for Cast Copper Nickel Grade |
Temperatura de fusión | 1100 - 1240 °C Show Material materials with Temperatura de fusión of 1100 - 1240 °C | Typical for Cast Copper Nickel Grade |
Chemical properties
Property | Value |
---|---|
Estaño | 7.5 - 8.5 % Show Material materials with Estaño of 7.5 - 8.5 % |
Manganeso | 0.05 - 0.3 % Show Material materials with Manganeso of 0.05 - 0.3 % |
Níquel | 14.5 - 15.5 % Show Material materials with Níquel of 14.5 - 15.5 % |
Plomo | 0.02 % Show Material materials with Plomo of 0.02 % |
Silicona | 0.3 % Show Material materials with Silicona of 0.3 % |
Zinc | 0.5 % Show Material materials with Zinc of 0.5 % |