General
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Densidad | 2.77 g/cm³ Show Material materials with Densidad of 2.77 g/cm³ | T8 | EN 573-3, EN 485, EN 754, EN 755 | Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar | |
20.0 °C | 2.77 g/cm³ Show Material materials with Densidad of 2.77 g/cm³ | T8 | EN 573-3 | Profile, Rod, Flat, Tube, Sheet |
Mecánica
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Bending Fatigue Strength | 125.0 MPa Show Material materials with Bending Fatigue Strength of 125.0 MPa | T8 | EN 573-3, EN 485, EN 754, EN 755 | Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar | ||
Coeficiente de Poisson | 0.33 [-] Show Material materials with Coeficiente de Poisson of 0.33 [-] | Typical for Wrought 2000 Series Aluminium | ||||
Dureza Brinell | 138.0 [-] Show Material materials with Dureza Brinell of 138.0 [-] | T8 | EN 573-3, EN 485 | Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar | ||
20.0 °C | 55.0 [-] Show Material materials with Dureza Brinell of 55.0 [-] | T8 | EN 573-3 | Tube | ||
20.0 °C | 115.0 [-] Show Material materials with Dureza Brinell of 115.0 [-] | T8 | EN 573-3 | Rod | ||
20.0 °C | 119.0 [-] Show Material materials with Dureza Brinell of 119.0 [-] | T8 | EN 573-3 | Rod | ||
20.0 °C | 130.0 [-] Show Material materials with Dureza Brinell of 130.0 [-] | T8 | EN 573-3 | Profile, Rod, Tube | ||
20.0 °C | 136.0 [-] Show Material materials with Dureza Brinell of 136.0 [-] | T8 | EN 573-3 | Sheet, Profile, Flat | ||
20.0 °C | 136.0 - 138.0 [-] Show Material materials with Dureza Brinell of 136.0 - 138.0 [-] | T8 | EN 573-3 | Flat | ||
20.0 °C | 136.0 - 137.0 [-] Show Material materials with Dureza Brinell of 136.0 - 137.0 [-] | T8 | EN 573-3 | Flat | ||
20.0 °C | 137.0 - 138.0 [-] Show Material materials with Dureza Brinell of 137.0 - 138.0 [-] | T8 | EN 573-3 | Flat | ||
20.0 °C | 137.0 [-] Show Material materials with Dureza Brinell of 137.0 [-] | T8 | EN 573-3 | Flat | ||
20.0 °C | 138.0 [-] Show Material materials with Dureza Brinell of 138.0 [-] | T8 | EN 573-3 | Flat | ||
Elongación | 3.0 % Show Material materials with Elongación of 3.0 % | T8 | EN 573-3, EN 754 | Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar | A50 | |
4.0 % Show Material materials with Elongación of 4.0 % | T8 | EN 573-3, EN 755 | Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar | A50 | ||
4.0 % Show Material materials with Elongación of 4.0 % | T8 | EN 573-3, EN 754 | Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar | A100 | ||
5.0 % Show Material materials with Elongación of 5.0 % | T8 | EN 573-3, EN 485 | Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar | A50 | ||
5.0 % Show Material materials with Elongación of 5.0 % | T8 | EN 573-3, EN 755 | Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar | A100 | ||
6.0 % Show Material materials with Elongación of 6.0 % | T8 | EN 573-3, EN 485 | Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar | A50 | ||
20.0 °C | 3.0 % Show Material materials with Elongación of 3.0 % | T8 | EN 573-3 | Rod | A50 | |
20.0 °C | 4.0 % Show Material materials with Elongación of 4.0 % | T8 | EN 573-3 | Sheet, Flat, Rod | ||
20.0 °C | 4.0 % Show Material materials with Elongación of 4.0 % | T8 | EN 573-3 | Profile, Rod, Tube | A50 | |
20.0 °C | 4.0 % Show Material materials with Elongación of 4.0 % | T8 | EN 573-3 | Flat | Transverse | |
20.0 °C | 5.0 % Show Material materials with Elongación of 5.0 % | T8 | EN 573-3 | Profile, Rod, Tube | ||
20.0 °C | 5.0 % Show Material materials with Elongación of 5.0 % | T8 | EN 573-3 | Flat | A50 | |
20.0 °C | 5.0 % Show Material materials with Elongación of 5.0 % | T8 | EN 573-3 | Flat | A50 Transverse | |
20.0 °C | 6.0 % Show Material materials with Elongación of 6.0 % | T8 | EN 573-3 | Flat | A50 | |
20.0 °C | 6.0 % Show Material materials with Elongación of 6.0 % | T8 | EN 573-3 | Flat | A50 Transverse | |
20.0 °C | 11.0 % Show Material materials with Elongación of 11.0 % | T8 | EN 573-3 | Transverse | ||
20.0 °C | 13.0 % Show Material materials with Elongación of 13.0 % | T8 | EN 573-3 | A50 Transverse | ||
Límite elástico | 380.0 MPa Show Material materials with Límite elástico of 380.0 MPa | T8 | EN 573-3, EN 755 | Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar | RP02 | |
400.0 MPa Show Material materials with Límite elástico of 400.0 MPa | T8 | EN 573-3, EN 485, EN 754 | Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar | RP02 | ||
20.0 °C | 290.0 MPa Show Material materials with Límite elástico of 290.0 MPa | T8 | EN 573-3 | RP02 Transverse | ||
20.0 °C | 380.0 MPa Show Material materials with Límite elástico of 380.0 MPa | T8 | EN 573-3 | Profile, Rod, Tube | RP02 | |
20.0 °C | 395.0 MPa Show Material materials with Límite elástico of 395.0 MPa | T8 | EN 573-3 | Sheet | RP02 | |
20.0 °C | 395.0 MPa Show Material materials with Límite elástico of 395.0 MPa | T8 | EN 573-3 | Flat | RP02 Transverse | |
20.0 °C | 400.0 MPa Show Material materials with Límite elástico of 400.0 MPa | T8 | EN 573-3 | Rod, Flat | RP02 | |
20.0 °C | 400.0 MPa Show Material materials with Límite elástico of 400.0 MPa | T8 | EN 573-3 | Flat | RP02 Transverse | |
20.0 °C | 450.0 MPa Show Material materials with Límite elástico of 450.0 MPa | T8 | EN 573-3 | Transverse | ||
20.0 °C | 450.0 MPa Show Material materials with Límite elástico of 450.0 MPa | T8 | EN 573-3 | |||
Módulo de cizallamiento | 27.4 GPa Show Material materials with Módulo de cizallamiento of 27.4 GPa | T8 | EN 573-3, EN 485, EN 754, EN 755 | Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar | ||
20.0 °C | 27.0 - 28.0 GPa Show Material materials with Módulo de cizallamiento of 27.0 - 28.0 GPa | T8 | EN 573-3 | Profile, Rod, Flat, Tube, Sheet | ||
Módulo elástico | 73.0 GPa Show Material materials with Módulo elástico of 73.0 GPa | T8 | EN 573-3, EN 485, EN 754, EN 755 | Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar | ||
20.0 °C | 70.0 - 74.5 GPa Show Material materials with Módulo elástico of 70.0 - 74.5 GPa | T8 | EN 573-3 | Profile, Rod, Flat, Tube, Sheet | ||
Plane-Strain Fracture Toughnes | 20.0 °C | 18.0 - 27.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 18.0 - 27.0 MPa·√m | T8 | EN 573-3 | ||
20.0 °C | 18.0 - 22.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 18.0 - 22.0 MPa·√m | T8 | EN 573-3 | |||
20.0 °C | 22.0 - 27.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 27.0 MPa·√m | T8 | EN 573-3 | |||
20.0 °C | 22.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 MPa·√m | T8 | EN 573-3 | |||
Resistencia a la tracción | 455.0 MPa Show Material materials with Resistencia a la tracción of 455.0 MPa | T8 | EN 573-3, EN 754, EN 755 | Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar | ||
460.0 MPa Show Material materials with Resistencia a la tracción of 460.0 MPa | T8 | EN 573-3, EN 485 | Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar | |||
20.0 °C | 430.0 MPa Show Material materials with Resistencia a la tracción of 430.0 MPa | T8 | EN 573-3 | Transverse | ||
20.0 °C | 440.0 MPa Show Material materials with Resistencia a la tracción of 440.0 MPa | T8 | EN 573-3 | Transverse | ||
20.0 °C | 455.0 MPa Show Material materials with Resistencia a la tracción of 455.0 MPa | T8 | EN 573-3 | Sheet, Profile, Rod, Tube, Flat | ||
20.0 °C | 455.0 MPa Show Material materials with Resistencia a la tracción of 455.0 MPa | T8 | EN 573-3 | Flat | Transverse | |
20.0 °C | 460.0 MPa Show Material materials with Resistencia a la tracción of 460.0 MPa | T8 | EN 573-3 | Flat | ||
20.0 °C | 460.0 MPa Show Material materials with Resistencia a la tracción of 460.0 MPa | T8 | EN 573-3 | Flat | Transverse | |
Ángulo de flexión a 90° | 5.0 °/t Show Material materials with Ángulo de flexión a 90° of 5.0 °/t | T8 | EN 573-3, EN 485 | Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar | ||
7.0 °/t Show Material materials with Ángulo de flexión a 90° of 7.0 °/t | T8 | EN 573-3, EN 485 | Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar |
Aplicaciones térmicas
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Calor específico | 875.0 J/(kg·K) Show Material materials with Calor específico of 875.0 J/(kg·K) | T8 | EN 573-3, EN 485, EN 754, EN 755 | Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar | |
20.0 °C | 875.0 J/(kg·K) Show Material materials with Calor específico of 875.0 J/(kg·K) | T8 | EN 573-3 | Profile, Rod, Flat, Tube, Sheet | |
Coeficiente de dilatación térmica | -50 °C | 2.11e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.11e-05 1/K | T8 | EN 573-3, EN 485, EN 754, EN 755 | Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar |
20 °C | 2.11e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.11e-05 1/K | T8 | EN 573-3, EN 485, EN 754, EN 755 | Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar | |
20 °C | 2.2899999999999998e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.2899999999999998e-05 1/K | T8 | EN 573-3, EN 485, EN 754, EN 755 | Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar | |
20 °C | 2.3199999999999998e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.3199999999999998e-05 1/K | T8 | EN 573-3, EN 485, EN 754, EN 755 | Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar | |
20 °C | 2.38e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.38e-05 1/K | T8 | EN 573-3, EN 485, EN 754, EN 755 | Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar | |
20 °C | 2.4699999999999997e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.4699999999999997e-05 1/K | T8 | EN 573-3, EN 485, EN 754, EN 755 | Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar | |
100 °C | 2.2899999999999998e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.2899999999999998e-05 1/K | T8 | EN 573-3, EN 485, EN 754, EN 755 | Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar | |
100 °C | 2.3199999999999998e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.3199999999999998e-05 1/K | T8 | EN 573-3, EN 485, EN 754, EN 755 | Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar | |
200 °C | 2.38e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.38e-05 1/K | T8 | EN 573-3, EN 485, EN 754, EN 755 | Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar | |
300 °C | 2.4699999999999997e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.4699999999999997e-05 1/K | T8 | EN 573-3, EN 485, EN 754, EN 755 | Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar | |
Conductividad térmica | 121.0 - 193.0 W/(m·K) Show Material materials with Conductividad térmica of 121.0 - 193.0 W/(m·K) | T8 | EN 573-3, EN 485, EN 754, EN 755 | Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar | |
20.0 °C | 130.0 - 150.0 W/(m·K) Show Material materials with Conductividad térmica of 130.0 - 150.0 W/(m·K) | T8 | EN 573-3, EN 485, EN 754, EN 755 | Profile, Rod, Flat, Tube, Sheet, Strip, Plate, Forging, Welded Tube, Bar | |
Temperatura de fusión | 505.0 - 640.0 °C Show Material materials with Temperatura de fusión of 505.0 - 640.0 °C | T8 | EN 573-3, EN 485, EN 754, EN 755 | Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar | |
505.0 - 635.0 °C Show Material materials with Temperatura de fusión of 505.0 - 635.0 °C | T8 | EN 573-3, EN 485, EN 754, EN 755 | Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar |
Eléctrico
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Conductividad eléctrica | 17000000.0 - 29000000.0 S/m Show Material materials with Conductividad eléctrica of 17000000.0 - 29000000.0 S/m | T8 | EN 573-3, EN 485, EN 754, EN 755 | Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar | |
20.0 °C | 18000000.0 - 21000000.0 S/m Show Material materials with Conductividad eléctrica of 18000000.0 - 21000000.0 S/m | T8 | EN 573-3, EN 485, EN 754, EN 755 | Profile, Rod, Flat, Tube, Sheet, Strip, Plate, Forging, Welded Tube, Bar | |
Resistividad eléctrica | 3.45e-08 - 5.88e-08 Ω·m Show Material materials with Resistividad eléctrica of 3.45e-08 - 5.88e-08 Ω·m | T8 | EN 573-3, EN 485, EN 754, EN 755 | Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar | |
4.76e-08 - 5.56e-08 Ω·m Show Material materials with Resistividad eléctrica of 4.76e-08 - 5.56e-08 Ω·m | T8 | EN 573-3, EN 485, EN 754, EN 755 | Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Cobre | 3.8 - 4.9 % Show Material materials with Cobre of 3.8 - 4.9 % | T8 | EN 573-3, EN 485, EN 754, EN 755 | Sheet, Flat, Profile, Rod, Tube, Strip, Plate, Forging, Welded Tube, Bar |
Cromo | 0.1 % Show Material materials with Cromo of 0.1 % | T8 | EN 573-3, EN 485, EN 754, EN 755 | Sheet, Flat, Profile, Rod, Tube, Strip, Plate, Forging, Welded Tube, Bar |
Hierro | 0.5 % Show Material materials with Hierro of 0.5 % | T8 | EN 573-3 | Sheet, Flat, Profile, Rod, Tube |
0.50 % Show Material materials with Hierro of 0.50 % | T8 | EN 573-3, EN 485, EN 754, EN 755 | Strip, Sheet, Plate, Forging, Tube, Welded Tube, Bar | |
Magnesio | 1.2 - 1.8 % Show Material materials with Magnesio of 1.2 - 1.8 % | T8 | EN 573-3, EN 485, EN 754, EN 755 | Sheet, Flat, Profile, Rod, Tube, Strip, Plate, Forging, Welded Tube, Bar |
Manganeso | 0.3 - 0.9 % Show Material materials with Manganeso of 0.3 - 0.9 % | T8 | EN 573-3, EN 485, EN 754, EN 755 | Sheet, Flat, Profile, Rod, Tube, Strip, Plate, Forging, Welded Tube, Bar |
Silicona | 0.5 % Show Material materials with Silicona of 0.5 % | T8 | EN 573-3, EN 485, EN 754, EN 755 | Sheet, Flat, Profile, Rod, Tube, Strip, Plate, Forging, Welded Tube, Bar |
Titanio | 0.15 % Show Material materials with Titanio of 0.15 % | T8 | EN 573-3, EN 485, EN 754, EN 755 | Sheet, Flat, Profile, Rod, Tube, Strip, Plate, Forging, Welded Tube, Bar |
Zinc | 0.25 % Show Material materials with Zinc of 0.25 % | T8 | EN 573-3, EN 485, EN 754, EN 755 | Sheet, Flat, Profile, Rod, Tube, Strip, Plate, Forging, Welded Tube, Bar |
Technological properties
Property | ||
---|---|---|
Anodizing | decorative: not suitable, Protective: good | |
Brazing | hard brazing (with flux/ without flux): not suitable / not suitable, friction soldering: acceptable, soft brazing with flux: not suitable | |
Corrosion properties | Seawater: poor, weathering: poor | |
Workability | Bending / Spinning (cold): sufficient (O) / acceptable (O), Impact extrusion (cold): acceptable (O), Deep drawing / upsetting (Condition) acceptable (O) / sufficient (O) |