General
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Densidad | 2.73 g/cm³ Show Material materials with Densidad of 2.73 g/cm³ | H22 | EN 573-3, EN 485, EN 546, EN 683 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | |
20.0 °C | 2.73 g/cm³ Show Material materials with Densidad of 2.73 g/cm³ | H22 | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541, EN 546-2, EN 683-2, EN 573-3 | Coil, Sheet, Foil, Foil, Flat, Plate |
Medidas
Property | Value | Condition | Related Standards | Thickness | Shape |
---|---|---|---|---|---|
Espesor | 0.2 mm Show Material materials with Espesor of 0.2 mm | H22 | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541, EN 546-2, EN 683-2 | 0.2 mm | Coil, Sheet, Foil |
1.0 mm Show Material materials with Espesor of 1.0 mm | H22 | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541, EN 546-2, EN 683-2 | 1.0 mm | Coil, Sheet, Foil |
Mecánica
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Bending Fatigue Strength | 55.0 MPa Show Material materials with Bending Fatigue Strength of 55.0 MPa | H22 | EN 573-3, EN 485, EN 546, EN 683 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | ||
Coeficiente de Poisson | 20.0 °C | 0.33 [-] Show Material materials with Coeficiente de Poisson of 0.33 [-] | H22 | EN 573-3 | Foil, Flat, Plate | |
Dureza Brinell | 37.0 [-] Show Material materials with Dureza Brinell of 37.0 [-] | H22 | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | ||
20.0 °C | 37.0 [-] Show Material materials with Dureza Brinell of 37.0 [-] | H22 | EN 573-3 | Flat | ||
Dureza Brinell (HBW) | 37.0 - 45.0 [-] Show Material materials with Dureza Brinell (HBW) of 37.0 - 45.0 [-] | H22 | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541, EN 546-2, EN 683-2 | Coil, Sheet, Foil | ||
Elongación | 4 % Show Material materials with Elongación of 4 % | H22 | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541, EN 546-2, EN 683-2 | Coil, Sheet, Foil | A50 | |
6.0 % Show Material materials with Elongación of 6.0 % | H22 | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | A50 | ||
7.0 % Show Material materials with Elongación of 7.0 % | H22 | EN 573-3, EN 485, EN 546 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | A50 | ||
8.0 % Show Material materials with Elongación of 8.0 % | H22 | EN 573-3, EN 485, EN 546, EN 683 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | A50 | ||
9.0 % Show Material materials with Elongación of 9.0 % | H22 | EN 573-3, EN 485, EN 683 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | A50 | ||
10.0 % Show Material materials with Elongación of 10.0 % | H22 | EN 573-3, EN 683 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | A50 | ||
11.0 % Show Material materials with Elongación of 11.0 % | H22 | EN 573-3, EN 485, EN 546 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | A50 | ||
14.0 % Show Material materials with Elongación of 14.0 % | H22 | EN 573-3, EN 546 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | A50 | ||
20.0 °C | 2.0 % Show Material materials with Elongación of 2.0 % | H22 | EN 573-3 | Plate | A50 | |
20.0 °C | 3.0 % Show Material materials with Elongación of 3.0 % | H22 | EN 573-3 | Plate | A50 | |
20.0 °C | 4.0 % Show Material materials with Elongación of 4.0 % | H22 | EN 573-3 | Plate | A50 | |
20.0 °C | 5.0 % Show Material materials with Elongación of 5.0 % | H22 | EN 573-3 | Foil | A100 | |
20.0 °C | 5.0 % Show Material materials with Elongación of 5.0 % | H22 | EN 573-3 | Foil, Plate | A50 | |
20.0 °C | 6.0 % Show Material materials with Elongación of 6.0 % | H22 | EN 573-3 | Foil | A100 | |
20.0 °C | 6.0 % Show Material materials with Elongación of 6.0 % | H22 | EN 573-3 | Foil, Plate, Flat | A50 | |
20.0 °C | 6.0 % Show Material materials with Elongación of 6.0 % | H22 | EN 573-3 | Flat | A50 Transverse | |
20.0 °C | 7.0 % Show Material materials with Elongación of 7.0 % | H22 | EN 573-3 | Foil | A100 | |
20.0 °C | 7.0 % Show Material materials with Elongación of 7.0 % | H22 | EN 573-3 | Foil, Flat | A50 | |
20.0 °C | 7.0 % Show Material materials with Elongación of 7.0 % | H22 | EN 573-3 | Flat | A50 Transverse | |
20.0 °C | 7.0 % Show Material materials with Elongación of 7.0 % | H22 | EN 573-3 | Plate | ||
20.0 °C | 8.0 % Show Material materials with Elongación of 8.0 % | H22 | EN 573-3 | Foil | A100 | |
20.0 °C | 8.0 % Show Material materials with Elongación of 8.0 % | H22 | EN 573-3 | Foil, Flat | A50 | |
20.0 °C | 8.0 % Show Material materials with Elongación of 8.0 % | H22 | EN 573-3 | Flat | A50 Transverse | |
20.0 °C | 9.0 % Show Material materials with Elongación of 9.0 % | H22 | EN 573-3 | Foil | A100 | |
20.0 °C | 9.0 % Show Material materials with Elongación of 9.0 % | H22 | EN 573-3 | Foil, Flat | A50 | |
20.0 °C | 9.0 % Show Material materials with Elongación of 9.0 % | H22 | EN 573-3 | Flat | A50 Transverse | |
20.0 °C | 10.0 % Show Material materials with Elongación of 10.0 % | H22 | EN 573-3 | Foil | A100 | |
20.0 °C | 10.0 % Show Material materials with Elongación of 10.0 % | H22 | EN 573-3 | Foil | A50 | |
20.0 °C | 10.0 % Show Material materials with Elongación of 10.0 % | H22 | EN 573-3 | Plate | ||
20.0 °C | 11.0 % Show Material materials with Elongación of 11.0 % | H22 | EN 573-3 | Foil | A100 | |
20.0 °C | 11.0 % Show Material materials with Elongación of 11.0 % | H22 | EN 573-3 | Foil, Flat | A50 | |
20.0 °C | 11.0 % Show Material materials with Elongación of 11.0 % | H22 | EN 573-3 | Flat | A50 Transverse | |
20.0 °C | 14.0 % Show Material materials with Elongación of 14.0 % | H22 | EN 573-3 | Foil | A100 | |
20.0 °C | 14.0 % Show Material materials with Elongación of 14.0 % | H22 | EN 573-3 | Foil | A50 | |
Límite elástico | 80.0 MPa Show Material materials with Límite elástico of 80.0 MPa | H22 | EN 573-3, EN 485, EN 683 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | RP02 | |
80 MPa Show Material materials with Límite elástico of 80 MPa | H22 | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541, EN 546-2, EN 683-2 | Coil, Sheet, Foil | |||
20.0 °C | 80.0 MPa Show Material materials with Límite elástico of 80.0 MPa | H22 | EN 573-3 | Flat | RP02 Transverse | |
20.0 °C | 80.0 MPa Show Material materials with Límite elástico of 80.0 MPa | H22 | EN 573-3 | Foil, Plate, Flat | RP02 | |
20.0 °C | 110.0 MPa Show Material materials with Límite elástico of 110.0 MPa | H22 | EN 573-3 | Plate | RP02 | |
20.0 °C | 115.0 MPa Show Material materials with Límite elástico of 115.0 MPa | H22 | EN 573-3 | Plate | RP02 | |
Módulo de cizallamiento | 26.0 GPa Show Material materials with Módulo de cizallamiento of 26.0 GPa | H22 | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541, EN 546-2, EN 683-2 | Coil, Sheet, Foil | ||
26.1 GPa Show Material materials with Módulo de cizallamiento of 26.1 GPa | H22 | EN 573-3, EN 485, EN 546, EN 683 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | |||
20.0 °C | 24.0 - 26.5 GPa Show Material materials with Módulo de cizallamiento of 24.0 - 26.5 GPa | H22 | EN 573-3 | Foil, Flat, Plate | ||
20.0 °C | 24.0 - 26.1 GPa Show Material materials with Módulo de cizallamiento of 24.0 - 26.1 GPa | H22 | EN 573-3 | Foil, Flat, Plate | ||
20.0 °C | 26.1 - 26.5 GPa Show Material materials with Módulo de cizallamiento of 26.1 - 26.5 GPa | H22 | EN 573-3 | Foil, Flat, Plate | ||
20.0 °C | 26.1 GPa Show Material materials with Módulo de cizallamiento of 26.1 GPa | H22 | EN 573-3 | Foil, Flat, Plate | ||
Módulo elástico | -270.0 °C | 70.0 GPa Show Material materials with Módulo elástico of 70.0 GPa | H22 | EN 573-3 | Foil, Flat, Plate | |
69.0 GPa Show Material materials with Módulo elástico of 69.0 GPa | H22 | EN 573-3, EN 485, EN 546, EN 683 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | |||
69.5 GPa Show Material materials with Módulo elástico of 69.5 GPa | H22 | EN 573-3, EN 485, EN 546, EN 683 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | |||
20.0 °C | 60.0 - 70.0 GPa Show Material materials with Módulo elástico of 60.0 - 70.0 GPa | H22 | EN 573-3 | Foil, Flat, Plate | ||
20.0 °C | 60.0 - 65.0 GPa Show Material materials with Módulo elástico of 60.0 - 65.0 GPa | H22 | EN 573-3 | Foil, Flat, Plate | ||
20.0 °C | 60.0 - 69.5 GPa Show Material materials with Módulo elástico of 60.0 - 69.5 GPa | H22 | EN 573-3 | Foil, Flat, Plate | ||
20.0 °C | 60.0 - 69.0 GPa Show Material materials with Módulo elástico of 60.0 - 69.0 GPa | H22 | EN 573-3 | Foil, Flat, Plate | ||
20.0 °C | 65.0 - 70.0 GPa Show Material materials with Módulo elástico of 65.0 - 70.0 GPa | H22 | EN 573-3 | Foil, Flat, Plate | ||
20.0 °C | 65.0 - 69.5 GPa Show Material materials with Módulo elástico of 65.0 - 69.5 GPa | H22 | EN 573-3 | Foil, Flat, Plate | ||
20.0 °C | 65.0 - 69.0 GPa Show Material materials with Módulo elástico of 65.0 - 69.0 GPa | H22 | EN 573-3 | Foil, Flat, Plate | ||
20.0 °C | 69.0 GPa Show Material materials with Módulo elástico of 69.0 GPa | H22 | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541, EN 546-2, EN 683-2, EN 573-3 | Coil, Sheet, Foil, Foil, Flat, Plate | ||
20.0 °C | 69.0 - 70.0 GPa Show Material materials with Módulo elástico of 69.0 - 70.0 GPa | H22 | EN 573-3 | Foil, Flat, Plate | ||
20.0 °C | 69.0 - 69.5 GPa Show Material materials with Módulo elástico of 69.0 - 69.5 GPa | H22 | EN 573-3 | Foil, Flat, Plate | ||
20.0 °C | 69.5 - 70.0 GPa Show Material materials with Módulo elástico of 69.5 - 70.0 GPa | H22 | EN 573-3 | Foil, Flat, Plate | ||
20.0 °C | 69.5 GPa Show Material materials with Módulo elástico of 69.5 GPa | H22 | EN 573-3 | Foil, Flat, Plate | ||
20.0 °C | 70.0 GPa Show Material materials with Módulo elástico of 70.0 GPa | H22 | EN 573-3 | Foil, Flat, Plate | ||
50.0 °C | 69.0 GPa Show Material materials with Módulo elástico of 69.0 GPa | H22 | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541, EN 546-2, EN 683-2, EN 573-3 | Coil, Sheet, Foil, Foil, Flat, Plate | ||
100.0 °C | 68.0 GPa Show Material materials with Módulo elástico of 68.0 GPa | H22 | EN 573-3 | Foil, Flat, Plate | ||
150.0 °C | 66.0 GPa Show Material materials with Módulo elástico of 66.0 GPa | H22 | EN 573-3 | Foil, Flat, Plate | ||
200.0 °C | 63.0 GPa Show Material materials with Módulo elástico of 63.0 GPa | H22 | EN 573-3 | Foil, Flat, Plate | ||
250.0 °C | 57.0 GPa Show Material materials with Módulo elástico of 57.0 GPa | H22 | EN 573-3 | Foil, Flat, Plate | ||
300.0 °C | 50.0 GPa Show Material materials with Módulo elástico of 50.0 GPa | H22 | EN 573-3 | Foil, Flat, Plate | ||
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 3000 Series Aluminium | ||||
Resistencia a la tracción | 120.0 - 185.0 MPa Show Material materials with Resistencia a la tracción of 120.0 - 185.0 MPa | H22 | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541, EN 546-2, EN 683-2 | Coil, Sheet, Foil | ||
20.0 °C | 120.0 - 160.0 MPa Show Material materials with Resistencia a la tracción of 120.0 - 160.0 MPa | H22 | EN 573-3, EN 485, EN 546, EN 683 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar, Flat | ||
20.0 °C | 120.0 - 180.0 MPa Show Material materials with Resistencia a la tracción of 120.0 - 180.0 MPa | H22 | EN 573-3 | Plate | ||
20.0 °C | 120.0 - 200.0 MPa Show Material materials with Resistencia a la tracción of 120.0 - 200.0 MPa | H22 | EN 573-3 | Plate | ||
20.0 °C | 120.0 - 160.0 MPa Show Material materials with Resistencia a la tracción of 120.0 - 160.0 MPa | H22 | EN 573-3 | Flat | Transverse | |
20.0 °C | 140.0 - 180.0 MPa Show Material materials with Resistencia a la tracción of 140.0 - 180.0 MPa | H22 | EN 573-3 | Plate | ||
20.0 °C | 140.0 - 200.0 MPa Show Material materials with Resistencia a la tracción of 140.0 - 200.0 MPa | H22 | EN 573-3 | Plate | ||
Ángulo de flexión a 180° | 1.0 °/t Show Material materials with Ángulo de flexión a 180° of 1.0 °/t | H22 | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | ||
1 °/t Show Material materials with Ángulo de flexión a 180° of 1 °/t | H22 | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541, EN 546-2, EN 683-2 | Coil, Sheet, Foil | |||
Ángulo de flexión a 90° | 0.5 °/t Show Material materials with Ángulo de flexión a 90° of 0.5 °/t | H22 | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | ||
0.5 °/t Show Material materials with Ángulo de flexión a 90° of 0.5 °/t | H22 | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541, EN 546-2, EN 683-2 | Coil, Sheet, Foil | |||
1.0 °/t Show Material materials with Ángulo de flexión a 90° of 1.0 °/t | H22 | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | |||
2.0 °/t Show Material materials with Ángulo de flexión a 90° of 2.0 °/t | H22 | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar |
Aplicaciones térmicas
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Calor específico | 893.0 J/(kg·K) Show Material materials with Calor específico of 893.0 J/(kg·K) | H22 | EN 573-3, EN 485, EN 546, EN 683 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | ||
20.0 °C | 892.0 - 893.0 J/(kg·K) Show Material materials with Calor específico of 892.0 - 893.0 J/(kg·K) | H22 | EN 573-3 | Foil, Flat, Plate | ||
20.0 °C | 892.0 J/(kg·K) Show Material materials with Calor específico of 892.0 J/(kg·K) | H22 | EN 573-3 | Foil, Flat, Plate | ||
20.0 °C | 893.0 J/(kg·K) Show Material materials with Calor específico of 893.0 J/(kg·K) | H22 | EN 573-3 | Foil, Flat, Plate | ||
Coeficiente de dilatación térmica | -50 °C | 2.1499999999999997e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.1499999999999997e-05 1/K | H22 | EN 573-3, EN 485, EN 546, EN 683 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | |
-50.0 °C | 2.15e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.15e-05 1/K | H22 | EN 573-3 | Foil, Flat, Plate | ||
20 °C | 2.1499999999999997e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.1499999999999997e-05 1/K | H22 | EN 573-3, EN 485, EN 546, EN 683 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | ||
20 °C | 2.3199999999999998e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.3199999999999998e-05 1/K | H22 | EN 573-3, EN 485, EN 546, EN 683 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | ||
20 °C | 2.41e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.41e-05 1/K | H22 | EN 573-3, EN 485, EN 546, EN 683 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar, Flat | ||
20 °C | 2.52e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.52e-05 1/K | H22 | EN 573-3, EN 485, EN 546, EN 683 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar, Flat | ||
100 °C | 0.000023 1/K Show Material materials with Coeficiente de dilatación térmica of 0.000023 1/K | H22 | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541, EN 546-2, EN 683-2 | Coil, Sheet, Foil | 20-100°C | |
100 °C | 2.3199999999999998e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.3199999999999998e-05 1/K | H22 | EN 573-3, EN 485, EN 546, EN 683 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | ||
100.0 °C | 2.32e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.32e-05 1/K | H22 | EN 573-3 | Foil, Flat, Plate | ||
200 °C | 2.41e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.41e-05 1/K | H22 | EN 573-3, EN 485, EN 546, EN 683 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar, Flat | ||
200.0 °C | 2.41e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.41e-05 1/K | H22 | EN 573-3, EN 485, EN 546, EN 683 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar, Flat | ||
300 °C | 2.52e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.52e-05 1/K | H22 | EN 573-3, EN 485, EN 546, EN 683 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar, Flat | ||
300.0 °C | 2.52e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.52e-05 1/K | H22 | EN 573-3, EN 485, EN 546, EN 683 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar, Flat | ||
Conductividad térmica | 159.0 - 193.0 W/(m·K) Show Material materials with Conductividad térmica of 159.0 - 193.0 W/(m·K) | H22 | EN 573-3, EN 485, EN 546, EN 683 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | ||
176 W/(m·K) Show Material materials with Conductividad térmica of 176 W/(m·K) | H22 | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541, EN 546-2, EN 683-2 | Coil, Sheet, Foil | |||
20.0 °C | 160.0 - 200.0 W/(m·K) Show Material materials with Conductividad térmica of 160.0 - 200.0 W/(m·K) | H22 | EN 573-3, EN 485, EN 546, EN 683 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar, Flat | ||
20.0 °C | 160.0 W/(m·K) Show Material materials with Conductividad térmica of 160.0 W/(m·K) | H22 | EN 573-3 | Foil, Flat, Plate | ||
Temperatura de fusión | 640.0 - 655.0 °C Show Material materials with Temperatura de fusión of 640.0 - 655.0 °C | H22 | EN 573-3, EN 485, EN 546, EN 683 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | ||
643.0 - 654.0 °C Show Material materials with Temperatura de fusión of 643.0 - 654.0 °C | H22 | EN 573-3, EN 485, EN 546, EN 683 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar |
Eléctrico
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Conductividad eléctrica | 24000000.0 - 29000000.0 S/m Show Material materials with Conductividad eléctrica of 24000000.0 - 29000000.0 S/m | H22 | EN 573-3, EN 485, EN 546, EN 683 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | |
20.0 °C | 22000000.0 - 29000000.0 S/m Show Material materials with Conductividad eléctrica of 22000000.0 - 29000000.0 S/m | H22 | EN 573-3 | Foil, Flat, Plate | |
20.0 °C | 23000000.0 - 29000000.0 S/m Show Material materials with Conductividad eléctrica of 23000000.0 - 29000000.0 S/m | H22 | EN 573-3, EN 485, EN 546, EN 683 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar, Flat | |
Resistividad eléctrica | 3.4e-08 Ω·m Show Material materials with Resistividad eléctrica of 3.4e-08 Ω·m | H22 | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541, EN 546-2, EN 683-2 | Coil, Sheet, Foil | |
3.45e-08 - 4.17e-08 Ω·m Show Material materials with Resistividad eléctrica of 3.45e-08 - 4.17e-08 Ω·m | H22 | EN 573-3, EN 485, EN 546, EN 683 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | ||
3.45e-08 - 4.35e-08 Ω·m Show Material materials with Resistividad eléctrica of 3.45e-08 - 4.35e-08 Ω·m | H22 | EN 573-3, EN 485, EN 546, EN 683 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | ||
20.0 °C | 3.4e-08 - 4.1e-08 Ω·m Show Material materials with Resistividad eléctrica of 3.4e-08 - 4.1e-08 Ω·m | H22 | EN 573-3 | Foil, Flat, Plate | |
20.0 °C | 3.4e-08 - 4.5e-08 Ω·m Show Material materials with Resistividad eléctrica of 3.4e-08 - 4.5e-08 Ω·m | H22 | EN 573-3 | Foil, Flat, Plate | |
20.0 °C | 4.1e-08 Ω·m Show Material materials with Resistividad eléctrica of 4.1e-08 Ω·m | H22 | EN 573-3 | Foil, Flat, Plate | |
20.0 °C | 4.1e-08 - 4.5e-08 Ω·m Show Material materials with Resistividad eléctrica of 4.1e-08 - 4.5e-08 Ω·m | H22 | EN 573-3 | Foil, Flat, Plate |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Cobre | 0.05 - 0.2 % Show Material materials with Cobre of 0.05 - 0.2 % | H22 | EN 573-3, EN 485, EN 546, EN 683, EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541, EN 546-2, EN 683-2 | Foil, Flat, Plate, Strip, Sheet, Wire, Tube, Bar, Coil, Sheet, Foil |
Hierro | 0.7 % Show Material materials with Hierro of 0.7 % | H22 | EN 573-3 | Foil, Flat, Plate |
0.70 % Show Material materials with Hierro of 0.70 % | H22 | EN 573-3, EN 485, EN 546, EN 683 | Strip, Sheet, Plate, Foil, Wire, Tube, Bar | |
0.7 % Show Material materials with Hierro of 0.7 % | H22 | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541, EN 546-2, EN 683-2 | Coil, Sheet, Foil | |
Manganeso | 1.0 - 1.5 % Show Material materials with Manganeso of 1.0 - 1.5 % | H22 | EN 573-3, EN 485, EN 546, EN 683, EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541, EN 546-2, EN 683-2 | Foil, Flat, Plate, Strip, Sheet, Wire, Tube, Bar, Coil, Sheet, Foil |
Silicona | 0.6 % Show Material materials with Silicona of 0.6 % | H22 | EN 573-3, EN 485, EN 546, EN 683 | Foil, Flat, Plate, Strip, Sheet, Wire, Tube, Bar |
0.6 % Show Material materials with Silicona of 0.6 % | H22 | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541, EN 546-2, EN 683-2 | Coil, Sheet, Foil | |
Zinc | 0.1 % Show Material materials with Zinc of 0.1 % | H22 | EN 573-3, EN 485, EN 546, EN 683 | Foil, Flat, Plate, Strip, Sheet, Wire, Tube, Bar |
0.1 % Show Material materials with Zinc of 0.1 % | H22 | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541, EN 546-2, EN 683-2 | Coil, Sheet, Foil |
Technological properties
Property | ||
---|---|---|
Anodizing | decorative: sufficient, Protective: very good | |
Application areas | Facades: Single sheet, Sheets for composites/ sandwich Panels, Sheets for mechanized panels; Roofing: Single sheet, Sheets for composites/ sandwich Panels; Doors: Sheets for composites/ sandwich Panels, Sheets for mechanized panels; Sun Protection Systems: Single sheet (covering, sun breakers and gutters); Interiors and ceilings: Single sheet, Sheets for composites/ sandwich Panels, Sheets for mechanized panels, Decoration; Furniture, Plinths, Blinds: Single sheet, Intermediate transformation/interior use; Anodizing Quality; Electronic devices: Housing of devices; Heat exchangers: Fins, Heat exchangers, General appliacations; Tubes: Industrial tubes, Flexible tube, Pipes; Wind energy: Nacelle coverings, Rotor, Hub, Stairs; Cosmetics: Cosmetics pieces; Semi-rigid and corrugated: Smooth wall; Automotive trim: Interior trims; Components: Heat shields, Automotive fins, Heat exchangers, General transportation | |
Brazing | hard brazing (with flux/ without flux): very good / very good, friction soldering: very good, soft brazing with flux: very good | |
Corrosion properties | Seawater: good, weathering: very good | |
Welding | Very Good | |
Workability | Bending / Spinning (cold): very good / very good, Impact extrusion (cold): acceptable, Deep drawing / upsetting (Condition) very good (O) / very good (H12) |