General
Property | Temperature | Value |
---|---|---|
Densidad | 20.0 °C | 7.83 g/cm³ Show Material materials with Densidad of 7.83 g/cm³ |
Mecánica
Property | Temperature | Value | Comment |
---|---|---|---|
Coeficiente de Poisson | 23.0 °C | 0.29 [-] Show Material materials with Coeficiente de Poisson of 0.29 [-] | Typical for Chromium Molybdenum Steel |
Elongación | 20.0 °C | 12 - 15 % Show Material materials with Elongación of 12 - 15 % | |
Estricción | 20.0 °C | 50 - 60 % Show Material materials with Estricción of 50 - 60 % | |
Límite elástico | 20.0 °C | 450 - 700 MPa Show Material materials with Límite elástico of 450 - 700 MPa | |
Módulo elástico | -100.0 °C | 217 GPa Show Material materials with Módulo elástico of 217 GPa | |
20.0 °C | 212 GPa Show Material materials with Módulo elástico of 212 GPa | ||
100.0 °C | 207 GPa Show Material materials with Módulo elástico of 207 GPa | ||
200.0 °C | 199 GPa Show Material materials with Módulo elástico of 199 GPa | ||
300.0 °C | 192 GPa Show Material materials with Módulo elástico of 192 GPa | ||
400.0 °C | 184 GPa Show Material materials with Módulo elástico of 184 GPa | ||
500.0 °C | 175 GPa Show Material materials with Módulo elástico of 175 GPa | ||
600.0 °C | 164 GPa Show Material materials with Módulo elástico of 164 GPa | ||
Resistencia a la tracción | 20.0 °C | 700 - 1100 MPa Show Material materials with Resistencia a la tracción of 700 - 1100 MPa |
Aplicaciones térmicas
Property | Temperature | Value | Comment |
---|---|---|---|
Calor específico | -100.0 °C | 423 J/(kg·K) Show Material materials with Calor específico of 423 J/(kg·K) | |
20.0 °C | 461 J/(kg·K) Show Material materials with Calor específico of 461 J/(kg·K) | ||
100.0 °C | 479 J/(kg·K) Show Material materials with Calor específico of 479 J/(kg·K) | ||
200.0 °C | 499 J/(kg·K) Show Material materials with Calor específico of 499 J/(kg·K) | ||
300.0 °C | 517 J/(kg·K) Show Material materials with Calor específico of 517 J/(kg·K) | ||
400.0 °C | 536 J/(kg·K) Show Material materials with Calor específico of 536 J/(kg·K) | ||
500.0 °C | 558 J/(kg·K) Show Material materials with Calor específico of 558 J/(kg·K) | ||
600.0 °C | 587 J/(kg·K) Show Material materials with Calor específico of 587 J/(kg·K) | ||
Coeficiente de dilatación térmica | -100.0 °C | 1.05E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.05E-5 1/K | |
20.0 °C | 1.15E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.15E-5 1/K | ||
100.0 °C | 1.21E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.21E-5 1/K | ||
200.0 °C | 1.27E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.27E-5 1/K | ||
300.0 °C | 1.32E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.32E-5 1/K | ||
400.0 °C | 1.36E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.36E-5 1/K | ||
500.0 °C | 1.4E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.4E-5 1/K | ||
600.0 °C | 1.44E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.44E-5 1/K | ||
Conductividad térmica | 20.0 °C | 41 W/(m·K) Show Material materials with Conductividad térmica of 41 W/(m·K) | |
100.0 °C | 42.7 W/(m·K) Show Material materials with Conductividad térmica of 42.7 W/(m·K) | ||
200.0 °C | 42.8 W/(m·K) Show Material materials with Conductividad térmica of 42.8 W/(m·K) | ||
300.0 °C | 41.6 W/(m·K) Show Material materials with Conductividad térmica of 41.6 W/(m·K) | ||
400.0 °C | 39.9 W/(m·K) Show Material materials with Conductividad térmica of 39.9 W/(m·K) | ||
500.0 °C | 37.8 W/(m·K) Show Material materials with Conductividad térmica of 37.8 W/(m·K) | ||
600.0 °C | 35.6 W/(m·K) Show Material materials with Conductividad térmica of 35.6 W/(m·K) | ||
Difusividad térmica | 20.0 °C | 11.4 mm²/s Show Material materials with Difusividad térmica of 11.4 mm²/s | |
100.0 °C | 11 mm²/s Show Material materials with Difusividad térmica of 11 mm²/s | ||
200.0 °C | 10.3 mm²/s Show Material materials with Difusividad térmica of 10.3 mm²/s | ||
300.0 °C | 9.5 mm²/s Show Material materials with Difusividad térmica of 9.5 mm²/s | ||
400.0 °C | 8.5 mm²/s Show Material materials with Difusividad térmica of 8.5 mm²/s | ||
500.0 °C | 7.3 mm²/s Show Material materials with Difusividad térmica of 7.3 mm²/s | ||
600.0 °C | 6 mm²/s Show Material materials with Difusividad térmica of 6 mm²/s | ||
Temperatura de fusión | 1382 - 1529 °C Show Material materials with Temperatura de fusión of 1382 - 1529 °C | Typical for Chromium Molybdenum Steel | |
Temperatura máx. de funcionamiento, largo | -40 - 0 °C Show Material materials with Temperatura máx. de funcionamiento, largo of -40 - 0 °C |
Eléctrico
Property | Temperature | Value |
---|---|---|
Resistividad eléctrica | 20.0 °C | 2.54E-7 Ω·m Show Material materials with Resistividad eléctrica of 2.54E-7 Ω·m |
100.0 °C | 3E-7 Ω·m Show Material materials with Resistividad eléctrica of 3E-7 Ω·m | |
200.0 °C | 3.69E-7 Ω·m Show Material materials with Resistividad eléctrica of 3.69E-7 Ω·m | |
300.0 °C | 4.51E-7 Ω·m Show Material materials with Resistividad eléctrica of 4.51E-7 Ω·m | |
400.0 °C | 5.45E-7 Ω·m Show Material materials with Resistividad eléctrica of 5.45E-7 Ω·m | |
500.0 °C | 6.54E-7 Ω·m Show Material materials with Resistividad eléctrica of 6.54E-7 Ω·m | |
600.0 °C | 7.78E-7 Ω·m Show Material materials with Resistividad eléctrica of 7.78E-7 Ω·m | |
Chemical properties
Property | Value |
---|---|
Azufre | 0.02 - 0.035 % Show Material materials with Azufre of 0.02 - 0.035 % |
Carbono | 0.22 - 0.29 % Show Material materials with Carbono of 0.22 - 0.29 % |
Cromo | 0.9 - 1.2 % Show Material materials with Cromo of 0.9 - 1.2 % |
Fósforo | 0.04 % Show Material materials with Fósforo of 0.04 % |
Manganeso | 0.6 - 0.9 % Show Material materials with Manganeso of 0.6 - 0.9 % |
Molibdeno | 0.15 - 0.3 % Show Material materials with Molibdeno of 0.15 - 0.3 % |
Silicona | 0.4 % Show Material materials with Silicona of 0.4 % |