General
Property | Temperature | Value |
---|---|---|
Densidad | 20.0 °C | 7.77 g/cm³ Show Material materials with Densidad of 7.77 g/cm³ |
Mecánica
Property | Temperature | Value |
---|---|---|
Coeficiente de Poisson | 20.0 °C | 0.3 [-] Show Material materials with Coeficiente de Poisson of 0.3 [-] |
95.0 °C | 0.3 [-] Show Material materials with Coeficiente de Poisson of 0.3 [-] | |
150.0 °C | 0.3 [-] Show Material materials with Coeficiente de Poisson of 0.3 [-] | |
205.0 °C | 0.3 [-] Show Material materials with Coeficiente de Poisson of 0.3 [-] | |
260.0 °C | 0.3 [-] Show Material materials with Coeficiente de Poisson of 0.3 [-] | |
315.0 °C | 0.3 [-] Show Material materials with Coeficiente de Poisson of 0.3 [-] | |
370.0 °C | 0.3 [-] Show Material materials with Coeficiente de Poisson of 0.3 [-] | |
425.0 °C | 0.3 [-] Show Material materials with Coeficiente de Poisson of 0.3 [-] | |
485.0 °C | 0.31 [-] Show Material materials with Coeficiente de Poisson of 0.31 [-] | |
540.0 °C | 0.31 [-] Show Material materials with Coeficiente de Poisson of 0.31 [-] | |
595.0 °C | 0.3 [-] Show Material materials with Coeficiente de Poisson of 0.3 [-] | |
650.0 °C | 0.33 [-] Show Material materials with Coeficiente de Poisson of 0.33 [-] | |
760.0 °C | 0.33 [-] Show Material materials with Coeficiente de Poisson of 0.33 [-] | |
Elongación | 20.0 °C | 20 % Show Material materials with Elongación of 20 % |
Elongación transversal | 20.0 °C | 18 % Show Material materials with Elongación transversal of 18 % |
Límite elástico Rp 0,2 | 20.0 °C | 390 MPa Show Material materials with Límite elástico Rp 0,2 of 390 MPa |
100.0 °C | 375 MPa Show Material materials with Límite elástico Rp 0,2 of 375 MPa | |
150.0 °C | 365 MPa Show Material materials with Límite elástico Rp 0,2 of 365 MPa | |
200.0 °C | 355 MPa Show Material materials with Límite elástico Rp 0,2 of 355 MPa | |
250.0 °C | 345 MPa Show Material materials with Límite elástico Rp 0,2 of 345 MPa | |
300.0 °C | 335 MPa Show Material materials with Límite elástico Rp 0,2 of 335 MPa | |
350.0 °C | 325 MPa Show Material materials with Límite elástico Rp 0,2 of 325 MPa | |
400.0 °C | 315 MPa Show Material materials with Límite elástico Rp 0,2 of 315 MPa | |
450.0 °C | 295 MPa Show Material materials with Límite elástico Rp 0,2 of 295 MPa | |
500.0 °C | 275 MPa Show Material materials with Límite elástico Rp 0,2 of 275 MPa | |
Límite elástico transversal Rp 0,2 | 20.0 °C | 390 MPa Show Material materials with Límite elástico transversal Rp 0,2 of 390 MPa |
Módulo de cizallamiento | 20.0 °C | 81.7 GPa Show Material materials with Módulo de cizallamiento of 81.7 GPa |
95.0 °C | 80.32 GPa Show Material materials with Módulo de cizallamiento of 80.32 GPa | |
150.0 °C | 78.95 GPa Show Material materials with Módulo de cizallamiento of 78.95 GPa | |
205.0 °C | 77.22 GPa Show Material materials with Módulo de cizallamiento of 77.22 GPa | |
260.0 °C | 75.5 GPa Show Material materials with Módulo de cizallamiento of 75.5 GPa | |
315.0 °C | 73.77 GPa Show Material materials with Módulo de cizallamiento of 73.77 GPa | |
370.0 °C | 71.71 GPa Show Material materials with Módulo de cizallamiento of 71.71 GPa | |
425.0 °C | 69.64 GPa Show Material materials with Módulo de cizallamiento of 69.64 GPa | |
485.0 °C | 67.22 GPa Show Material materials with Módulo de cizallamiento of 67.22 GPa | |
540.0 °C | 65.16 GPa Show Material materials with Módulo de cizallamiento of 65.16 GPa | |
595.0 °C | 63.43 GPa Show Material materials with Módulo de cizallamiento of 63.43 GPa | |
650.0 °C | 60.33 GPa Show Material materials with Módulo de cizallamiento of 60.33 GPa | |
760.0 °C | 51.71 GPa Show Material materials with Módulo de cizallamiento of 51.71 GPa | |
Módulo elástico | 20.0 °C | 211.67 - 218 GPa Show Material materials with Módulo elástico of 211.67 - 218 GPa |
95.0 °C | 208.22 GPa Show Material materials with Módulo elástico of 208.22 GPa | |
100.0 °C | 213 - 214 GPa Show Material materials with Módulo elástico of 213 - 214 GPa | |
150.0 °C | 204.77 GPa Show Material materials with Módulo elástico of 204.77 GPa | |
200.0 °C | 206 - 207 GPa Show Material materials with Módulo elástico of 206 - 207 GPa | |
205.0 °C | 200.64 GPa Show Material materials with Módulo elástico of 200.64 GPa | |
260.0 °C | 196.5 GPa Show Material materials with Módulo elástico of 196.5 GPa | |
300.0 °C | 198 - 199 GPa Show Material materials with Módulo elástico of 198 - 199 GPa | |
315.0 °C | 191.67 GPa Show Material materials with Módulo elástico of 191.67 GPa | |
370.0 °C | 186.85 GPa Show Material materials with Módulo elástico of 186.85 GPa | |
400.0 °C | 190 GPa Show Material materials with Módulo elástico of 190 GPa | |
425.0 °C | 181.33 GPa Show Material materials with Módulo elástico of 181.33 GPa | |
485.0 °C | 175.82 GPa Show Material materials with Módulo elástico of 175.82 GPa | |
500.0 °C | 180 GPa Show Material materials with Módulo elástico of 180 GPa | |
540.0 °C | 170.3 GPa Show Material materials with Módulo elástico of 170.3 GPa | |
595.0 °C | 165.47 GPa Show Material materials with Módulo elástico of 165.47 GPa | |
600.0 °C | 167 - 168 GPa Show Material materials with Módulo elástico of 167 - 168 GPa | |
650.0 °C | 159.96 GPa Show Material materials with Módulo elástico of 159.96 GPa | |
700.0 °C | 150 GPa Show Material materials with Módulo elástico of 150 GPa | |
760.0 °C | 137.21 GPa Show Material materials with Módulo elástico of 137.21 GPa | |
Resistencia a la tracción | 20.0 °C | 590 - 740 MPa Show Material materials with Resistencia a la tracción of 590 - 740 MPa |
100.0 °C | 550 MPa Show Material materials with Resistencia a la tracción of 550 MPa | |
150.0 °C | 525 MPa Show Material materials with Resistencia a la tracción of 525 MPa | |
200.0 °C | 500 MPa Show Material materials with Resistencia a la tracción of 500 MPa | |
250.0 °C | 490 MPa Show Material materials with Resistencia a la tracción of 490 MPa | |
300.0 °C | 480 MPa Show Material materials with Resistencia a la tracción of 480 MPa | |
350.0 °C | 460 MPa Show Material materials with Resistencia a la tracción of 460 MPa | |
400.0 °C | 430 MPa Show Material materials with Resistencia a la tracción of 430 MPa | |
450.0 °C | 405 MPa Show Material materials with Resistencia a la tracción of 405 MPa | |
500.0 °C | 360 MPa Show Material materials with Resistencia a la tracción of 360 MPa | |
Resistencia a la tracción transversal | 20.0 °C | 590 - 740 MPa Show Material materials with Resistencia a la tracción transversal of 590 - 740 MPa |
Aplicaciones térmicas
Property | Temperature | Value | Comment |
---|---|---|---|
Calor específico | 20.0 °C | 429 J/(kg·K) Show Material materials with Calor específico of 429 J/(kg·K) | |
100.0 °C | 464 - 500 J/(kg·K) Show Material materials with Calor específico of 464 - 500 J/(kg·K) | ||
200.0 °C | 492 - 530 J/(kg·K) Show Material materials with Calor específico of 492 - 530 J/(kg·K) | ||
300.0 °C | 511 - 560 J/(kg·K) Show Material materials with Calor específico of 511 - 560 J/(kg·K) | ||
400.0 °C | 531 - 610 J/(kg·K) Show Material materials with Calor específico of 531 - 610 J/(kg·K) | ||
500.0 °C | 554 - 680 J/(kg·K) Show Material materials with Calor específico of 554 - 680 J/(kg·K) | ||
600.0 °C | 585 - 780 J/(kg·K) Show Material materials with Calor específico of 585 - 780 J/(kg·K) | ||
700.0 °C | 626 J/(kg·K) Show Material materials with Calor específico of 626 J/(kg·K) | ||
Coeficiente de dilatación térmica | -100.0 °C | 1E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1E-5 1/K | |
20.0 °C | 1.08E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.08E-5 1/K | ||
100.0 °C | 1.12E-5 - 1.13E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.12E-5 - 1.13E-5 1/K | ||
200.0 °C | 1.16E-5 - 1.18E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.16E-5 - 1.18E-5 1/K | ||
300.0 °C | 1.2E-5 - 1.23E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.2E-5 - 1.23E-5 1/K | ||
400.0 °C | 1.23E-5 - 1.27E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.23E-5 - 1.27E-5 1/K | ||
425.0 °C | 1.19E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.19E-5 1/K | ||
485.0 °C | 1.22E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.22E-5 1/K | ||
500.0 °C | 1.26E-5 - 1.3E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.26E-5 - 1.3E-5 1/K | ||
540.0 °C | 1.23E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.23E-5 1/K | ||
595.0 °C | 1.25E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.25E-5 1/K | ||
600.0 °C | 1.29E-5 - 1.32E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.29E-5 - 1.32E-5 1/K | ||
650.0 °C | 1.27E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.27E-5 1/K | ||
700.0 °C | 1.33E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.33E-5 1/K | ||
Conductividad térmica | 20.0 °C | 20.7 W/(m·K) Show Material materials with Conductividad térmica of 20.7 W/(m·K) | |
100.0 °C | 22.6 - 23 W/(m·K) Show Material materials with Conductividad térmica of 22.6 - 23 W/(m·K) | ||
200.0 °C | 24 - 24.4 W/(m·K) Show Material materials with Conductividad térmica of 24 - 24.4 W/(m·K) | ||
300.0 °C | 25.8 - 26 W/(m·K) Show Material materials with Conductividad térmica of 25.8 - 26 W/(m·K) | ||
400.0 °C | 26.9 - 27 W/(m·K) Show Material materials with Conductividad térmica of 26.9 - 27 W/(m·K) | ||
500.0 °C | 27.8 - 28 W/(m·K) Show Material materials with Conductividad térmica of 27.8 - 28 W/(m·K) | ||
600.0 °C | 28.5 - 29 W/(m·K) Show Material materials with Conductividad térmica of 28.5 - 29 W/(m·K) | ||
700.0 °C | 28.8 W/(m·K) Show Material materials with Conductividad térmica of 28.8 W/(m·K) | ||
Difusividad térmica | 20.0 °C | 6.2 mm²/s Show Material materials with Difusividad térmica of 6.2 mm²/s | |
100.0 °C | 5.9 mm²/s Show Material materials with Difusividad térmica of 5.9 mm²/s | ||
200.0 °C | 6 mm²/s Show Material materials with Difusividad térmica of 6 mm²/s | ||
300.0 °C | 6 mm²/s Show Material materials with Difusividad térmica of 6 mm²/s | ||
400.0 °C | 5.7 mm²/s Show Material materials with Difusividad térmica of 5.7 mm²/s | ||
500.0 °C | 5.4 mm²/s Show Material materials with Difusividad térmica of 5.4 mm²/s | ||
600.0 °C | 4.8 mm²/s Show Material materials with Difusividad térmica of 4.8 mm²/s | ||
700.0 °C | 4 mm²/s Show Material materials with Difusividad térmica of 4 mm²/s | ||
Temperatura de fusión | 1382 - 1529 °C Show Material materials with Temperatura de fusión of 1382 - 1529 °C | Typical for Chromium Molybdenum Steel |
Eléctrico
Property | Temperature | Value |
---|---|---|
Resistividad eléctrica | 20.0 °C | 5.03E-7 Ω·m Show Material materials with Resistividad eléctrica of 5.03E-7 Ω·m |
100.0 °C | 5.67E-7 - 5.7E-7 Ω·m Show Material materials with Resistividad eléctrica of 5.67E-7 - 5.7E-7 Ω·m | |
200.0 °C | 6.47E-7 - 6.5E-7 Ω·m Show Material materials with Resistividad eléctrica of 6.47E-7 - 6.5E-7 Ω·m | |
300.0 °C | 7.27E-7 - 7.3E-7 Ω·m Show Material materials with Resistividad eléctrica of 7.27E-7 - 7.3E-7 Ω·m | |
400.0 °C | 8.09E-7 - 8.1E-7 Ω·m Show Material materials with Resistividad eléctrica of 8.09E-7 - 8.1E-7 Ω·m | |
500.0 °C | 8.9E-7 Ω·m Show Material materials with Resistividad eléctrica of 8.9E-7 Ω·m | |
600.0 °C | 9.7E-7 - 9.72E-7 Ω·m Show Material materials with Resistividad eléctrica of 9.7E-7 - 9.72E-7 Ω·m | |
700.0 °C | 1.06E-6 Ω·m Show Material materials with Resistividad eléctrica of 1.06E-6 Ω·m | |
Chemical properties
Property | Value |
---|---|
Azufre | 0.03 % Show Material materials with Azufre of 0.03 % |
Carbono | 0.15 % Show Material materials with Carbono of 0.15 % |
Cromo | 8 - 10 % Show Material materials with Cromo of 8 - 10 % |
Fósforo | 0.03 % Show Material materials with Fósforo of 0.03 % |
Manganeso | 0.3 - 0.6 % Show Material materials with Manganeso of 0.3 - 0.6 % |
Molibdeno | 0.9 - 1.1 % Show Material materials with Molibdeno of 0.9 - 1.1 % |
Silicona | 0.25 - 1 % Show Material materials with Silicona of 0.25 - 1 % |