DIN 1654-5 Grade X2CrNiN18-10 cold drawn and quenched

View suppliers (1)
Want to keep this datasheet? Save it now in your required format

Description

X 2 CrNi 18 10 is an austenitic CrNi steel which, due to the added nitrogen alloy, possesses an increased yield strength which also persist in higher temperatures. It is suitable for the chemical equipment construction because of its resistance to nitric acid. The steel is well suited for cold-forming and can undergo high-gloss polishing. It is used for screws, nuts and molded parts at temperatures from -270 up to 400 degrees C.

Related Standards

Equivalent Materials

Los datos sobre este material han sido proporcionados por WIAM.

A menos que se indique lo contrario, todas las medidas corresponden a condiciones de temperatura ambiente. A menos que se indique lo contrario, se utilizan las unidades del SI.
Las normas armonizadas son similares a uno o varios estándares del proveedor. Es posible que algunas normas armonizadas se ajusten al estándar original, mientras que otras pueden quedar fuera de su alcance.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Propiedades

General

PropertyTemperatureValue

Densidad

20.0 °C

7.93 g/cm³

Show Material materials with Densidad of 7.93 g/cm³

Mecánica

PropertyTemperatureValueComment

Coeficiente de Poisson

23.0 °C

0.3 [-]

Show Material materials with Coeficiente de Poisson of 0.3 [-]

Typical for Austenitic Stainless Steel

Estricción

20.0 °C

55 %

Show Material materials with Estricción of 55 %

Módulo de cizallamiento

23.0 °C

77 GPa

Show Material materials with Módulo de cizallamiento of 77 GPa

Typical for Austenitic Stainless Steel

Módulo elástico

-100.0 °C

206 GPa

Show Material materials with Módulo elástico of 206 GPa

20.0 °C

196 GPa

Show Material materials with Módulo elástico of 196 GPa

100.0 °C

190 - 194 GPa

Show Material materials with Módulo elástico of 190 - 194 GPa

200.0 °C

182 - 186 GPa

Show Material materials with Módulo elástico of 182 - 186 GPa

300.0 °C

174 - 179 GPa

Show Material materials with Módulo elástico of 174 - 179 GPa

400.0 °C

166 - 172 GPa

Show Material materials with Módulo elástico of 166 - 172 GPa

500.0 °C

158 - 165 GPa

Show Material materials with Módulo elástico of 158 - 165 GPa

600.0 °C

150 GPa

Show Material materials with Módulo elástico of 150 GPa

700.0 °C

142 GPa

Show Material materials with Módulo elástico of 142 GPa

800.0 °C

134 GPa

Show Material materials with Módulo elástico of 134 GPa

900.0 °C

127 GPa

Show Material materials with Módulo elástico of 127 GPa

1000.0 °C

120 GPa

Show Material materials with Módulo elástico of 120 GPa

Resistencia a la tracción

20.0 °C

730 MPa

Show Material materials with Resistencia a la tracción of 730 MPa

Aplicaciones térmicas

PropertyTemperatureValueComment

Calor específico

-100.0 °C

440 J/(kg·K)

Show Material materials with Calor específico of 440 J/(kg·K)

20.0 °C

472 J/(kg·K)

Show Material materials with Calor específico of 472 J/(kg·K)

100.0 °C

487 J/(kg·K)

Show Material materials with Calor específico of 487 J/(kg·K)

200.0 °C

503 J/(kg·K)

Show Material materials with Calor específico of 503 J/(kg·K)

300.0 °C

512 J/(kg·K)

Show Material materials with Calor específico of 512 J/(kg·K)

400.0 °C

520 J/(kg·K)

Show Material materials with Calor específico of 520 J/(kg·K)

500.0 °C

530 J/(kg·K)

Show Material materials with Calor específico of 530 J/(kg·K)

600.0 °C

541 J/(kg·K)

Show Material materials with Calor específico of 541 J/(kg·K)

700.0 °C

551 J/(kg·K)

Show Material materials with Calor específico of 551 J/(kg·K)

800.0 °C

559 J/(kg·K)

Show Material materials with Calor específico of 559 J/(kg·K)

900.0 °C

565 J/(kg·K)

Show Material materials with Calor específico of 565 J/(kg·K)

1000.0 °C

571 J/(kg·K)

Show Material materials with Calor específico of 571 J/(kg·K)

Unlock all property charts

Coeficiente de dilatación térmica

-100.0 °C

1.49E-5 1/K

Show Material materials with Coeficiente de dilatación térmica of 1.49E-5 1/K

20.0 °C

1.61E-5 1/K

Show Material materials with Coeficiente de dilatación térmica of 1.61E-5 1/K

100.0 °C

1.6E-5 - 1.67E-5 1/K

Show Material materials with Coeficiente de dilatación térmica of 1.6E-5 - 1.67E-5 1/K

200.0 °C

1.7E-5 - 1.72E-5 1/K

Show Material materials with Coeficiente de dilatación térmica of 1.7E-5 - 1.72E-5 1/K

300.0 °C

1.7E-5 - 1.77E-5 1/K

Show Material materials with Coeficiente de dilatación térmica of 1.7E-5 - 1.77E-5 1/K

400.0 °C

1.8E-5 - 1.81E-5 1/K

Show Material materials with Coeficiente de dilatación térmica of 1.8E-5 - 1.81E-5 1/K

500.0 °C

1.8E-5 - 1.84E-5 1/K

Show Material materials with Coeficiente de dilatación térmica of 1.8E-5 - 1.84E-5 1/K

600.0 °C

1.88E-5 1/K

Show Material materials with Coeficiente de dilatación térmica of 1.88E-5 1/K

700.0 °C

1.91E-5 1/K

Show Material materials with Coeficiente de dilatación térmica of 1.91E-5 1/K

800.0 °C

1.94E-5 1/K

Show Material materials with Coeficiente de dilatación térmica of 1.94E-5 1/K

900.0 °C

1.97E-5 1/K

Show Material materials with Coeficiente de dilatación térmica of 1.97E-5 1/K

1000.0 °C

2E-5 1/K

Show Material materials with Coeficiente de dilatación térmica of 2E-5 1/K

Unlock all property charts

Conductividad térmica

20.0 °C

14.3 W/(m·K)

Show Material materials with Conductividad térmica of 14.3 W/(m·K)

100.0 °C

15.8 W/(m·K)

Show Material materials with Conductividad térmica of 15.8 W/(m·K)

200.0 °C

17.5 W/(m·K)

Show Material materials with Conductividad térmica of 17.5 W/(m·K)

300.0 °C

19 W/(m·K)

Show Material materials with Conductividad térmica of 19 W/(m·K)

400.0 °C

20.5 W/(m·K)

Show Material materials with Conductividad térmica of 20.5 W/(m·K)

500.0 °C

21.9 W/(m·K)

Show Material materials with Conductividad térmica of 21.9 W/(m·K)

600.0 °C

23.3 W/(m·K)

Show Material materials with Conductividad térmica of 23.3 W/(m·K)

700.0 °C

24.6 W/(m·K)

Show Material materials with Conductividad térmica of 24.6 W/(m·K)

800.0 °C

26 W/(m·K)

Show Material materials with Conductividad térmica of 26 W/(m·K)

900.0 °C

27.4 W/(m·K)

Show Material materials with Conductividad térmica of 27.4 W/(m·K)

1000.0 °C

28.8 W/(m·K)

Show Material materials with Conductividad térmica of 28.8 W/(m·K)

Unlock all property charts

Difusividad térmica

20.0 °C

3.8 mm²/s

Show Material materials with Difusividad térmica of 3.8 mm²/s

100.0 °C

4 mm²/s

Show Material materials with Difusividad térmica of 4 mm²/s

200.0 °C

4.2 mm²/s

Show Material materials with Difusividad térmica of 4.2 mm²/s

300.0 °C

4.6 mm²/s

Show Material materials with Difusividad térmica of 4.6 mm²/s

400.0 °C

4.8 mm²/s

Show Material materials with Difusividad térmica of 4.8 mm²/s

500.0 °C

4.9 mm²/s

Show Material materials with Difusividad térmica of 4.9 mm²/s

600.0 °C

5 mm²/s

Show Material materials with Difusividad térmica of 5 mm²/s

700.0 °C

5.3 mm²/s

Show Material materials with Difusividad térmica of 5.3 mm²/s

800.0 °C

5.6 mm²/s

Show Material materials with Difusividad térmica of 5.6 mm²/s

900.0 °C

5.9 mm²/s

Show Material materials with Difusividad térmica of 5.9 mm²/s

1000.0 °C

6 mm²/s

Show Material materials with Difusividad térmica of 6 mm²/s

Unlock all property charts

Temperatura de fusión

1230 - 1480 °C

Show Material materials with Temperatura de fusión of 1230 - 1480 °C

Typical for Austenitic Stainless Steel

Temperatura máx. de funcionamiento, largo

-270 - 400 °C

Show Material materials with Temperatura máx. de funcionamiento, largo of -270 - 400 °C

Eléctrico

PropertyTemperatureValue

Resistividad eléctrica

20.0 °C

7.1E-7 Ω·m

Show Material materials with Resistividad eléctrica of 7.1E-7 Ω·m

100.0 °C

7.76E-7 Ω·m

Show Material materials with Resistividad eléctrica of 7.76E-7 Ω·m

200.0 °C

8.49E-7 Ω·m

Show Material materials with Resistividad eléctrica of 8.49E-7 Ω·m

300.0 °C

9.14E-7 Ω·m

Show Material materials with Resistividad eléctrica of 9.14E-7 Ω·m

400.0 °C

9.71E-7 Ω·m

Show Material materials with Resistividad eléctrica of 9.71E-7 Ω·m

500.0 °C

1.02E-6 Ω·m

Show Material materials with Resistividad eléctrica of 1.02E-6 Ω·m

600.0 °C

1.07E-6 Ω·m

Show Material materials with Resistividad eléctrica of 1.07E-6 Ω·m

700.0 °C

1.1E-6 Ω·m

Show Material materials with Resistividad eléctrica of 1.1E-6 Ω·m

800.0 °C

1.14E-6 Ω·m

Show Material materials with Resistividad eléctrica of 1.14E-6 Ω·m

900.0 °C

1.17E-6 Ω·m

Show Material materials with Resistividad eléctrica of 1.17E-6 Ω·m

1000.0 °C

1.19E-6 Ω·m

Show Material materials with Resistividad eléctrica of 1.19E-6 Ω·m

Unlock all property charts

Chemical properties

PropertyValue

Azufre

0.03 %

Show Material materials with Azufre of 0.03 %

Carbono

0.03 %

Show Material materials with Carbono of 0.03 %

Cromo

17 - 19 %

Show Material materials with Cromo of 17 - 19 %

Fósforo

0.05 %

Show Material materials with Fósforo of 0.05 %

Manganeso

2 %

Show Material materials with Manganeso of 2 %

Níquel

8.5 - 11.5 %

Show Material materials with Níquel of 8.5 - 11.5 %

Silicona

1 %

Show Material materials with Silicona of 1 %