General
Property | Temperature | Value |
---|---|---|
Densidad | 20.0 °C | 7.58 - 7.7 g/cm³ Show Material materials with Densidad of 7.58 - 7.7 g/cm³ |
Mecánica
Property | Temperature | Value | Comment |
---|---|---|---|
Coeficiente de Poisson | 23.0 °C | 0.3 [-] Show Material materials with Coeficiente de Poisson of 0.3 [-] | Typical for Martensitic Stainless Steel |
Dureza Brinell | 20.0 °C | 240 - 290 [-] Show Material materials with Dureza Brinell of 240 - 290 [-] | |
Elongación | 20.0 °C | 17 % Show Material materials with Elongación of 17 % | |
Elongación transversal | 20.0 °C | 16 % Show Material materials with Elongación transversal of 16 % | |
Límite elástico Rp 0,2 | 20.0 °C | 550 MPa Show Material materials with Límite elástico Rp 0,2 of 550 MPa | |
50.0 °C | 540 MPa Show Material materials with Límite elástico Rp 0,2 of 540 MPa | ||
100.0 °C | 530 MPa Show Material materials with Límite elástico Rp 0,2 of 530 MPa | ||
150.0 °C | 515 MPa Show Material materials with Límite elástico Rp 0,2 of 515 MPa | ||
200.0 °C | 500 MPa Show Material materials with Límite elástico Rp 0,2 of 500 MPa | ||
250.0 °C | 490 MPa Show Material materials with Límite elástico Rp 0,2 of 490 MPa | ||
300.0 °C | 475 MPa Show Material materials with Límite elástico Rp 0,2 of 475 MPa | ||
Límite elástico transversal Rp 0,2 | 20.0 °C | 550 MPa Show Material materials with Límite elástico transversal Rp 0,2 of 550 MPa | |
Módulo de cizallamiento | 23.0 °C | 77 GPa Show Material materials with Módulo de cizallamiento of 77 GPa | Typical for Martensitic Stainless Steel |
Módulo elástico | 20.0 °C | 198 - 218 GPa Show Material materials with Módulo elástico of 198 - 218 GPa | |
100.0 °C | 193 - 213 GPa Show Material materials with Módulo elástico of 193 - 213 GPa | ||
200.0 °C | 183 - 206 GPa Show Material materials with Módulo elástico of 183 - 206 GPa | ||
300.0 °C | 175 - 198 GPa Show Material materials with Módulo elástico of 175 - 198 GPa | ||
400.0 °C | 172 - 190 GPa Show Material materials with Módulo elástico of 172 - 190 GPa | ||
500.0 °C | 159 - 180 GPa Show Material materials with Módulo elástico of 159 - 180 GPa | ||
600.0 °C | 167 GPa Show Material materials with Módulo elástico of 167 GPa | ||
700.0 °C | 150 GPa Show Material materials with Módulo elástico of 150 GPa | ||
Resistencia a la tracción | 20.0 °C | 760 - 900 MPa Show Material materials with Resistencia a la tracción of 760 - 900 MPa | |
Resistencia a la tracción transversal | 20.0 °C | 760 - 900 MPa Show Material materials with Resistencia a la tracción transversal of 760 - 900 MPa |
Aplicaciones térmicas
Property | Temperature | Value | Comment |
---|---|---|---|
Calor específico | 20.0 °C | 430 - 439 J/(kg·K) Show Material materials with Calor específico of 430 - 439 J/(kg·K) | |
100.0 °C | 474 J/(kg·K) Show Material materials with Calor específico of 474 J/(kg·K) | ||
200.0 °C | 492 J/(kg·K) Show Material materials with Calor específico of 492 J/(kg·K) | ||
300.0 °C | 517 J/(kg·K) Show Material materials with Calor específico of 517 J/(kg·K) | ||
400.0 °C | 538 J/(kg·K) Show Material materials with Calor específico of 538 J/(kg·K) | ||
500.0 °C | 564 J/(kg·K) Show Material materials with Calor específico of 564 J/(kg·K) | ||
600.0 °C | 598 J/(kg·K) Show Material materials with Calor específico of 598 J/(kg·K) | ||
700.0 °C | 647 J/(kg·K) Show Material materials with Calor específico of 647 J/(kg·K) | ||
Coeficiente de dilatación térmica | 20.0 °C | 1.02E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.02E-5 1/K | |
100.0 °C | 1.05E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.05E-5 1/K | ||
200.0 °C | 1.09E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.09E-5 1/K | ||
300.0 °C | 1.13E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.13E-5 1/K | ||
400.0 °C | 1.16E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.16E-5 1/K | ||
500.0 °C | 1.2E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.2E-5 1/K | ||
600.0 °C | 1.22E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.22E-5 1/K | ||
700.0 °C | 1.24E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.24E-5 1/K | ||
Conductividad térmica | 20.0 °C | 15.7 - 25 W/(m·K) Show Material materials with Conductividad térmica of 15.7 - 25 W/(m·K) | |
100.0 °C | 17.1 W/(m·K) Show Material materials with Conductividad térmica of 17.1 W/(m·K) | ||
200.0 °C | 18.6 W/(m·K) Show Material materials with Conductividad térmica of 18.6 W/(m·K) | ||
300.0 °C | 20 W/(m·K) Show Material materials with Conductividad térmica of 20 W/(m·K) | ||
400.0 °C | 21.2 W/(m·K) Show Material materials with Conductividad térmica of 21.2 W/(m·K) | ||
500.0 °C | 22.3 W/(m·K) Show Material materials with Conductividad térmica of 22.3 W/(m·K) | ||
600.0 °C | 23.1 W/(m·K) Show Material materials with Conductividad térmica of 23.1 W/(m·K) | ||
700.0 °C | 23.8 W/(m·K) Show Material materials with Conductividad térmica of 23.8 W/(m·K) | ||
Difusividad térmica | 20.0 °C | 4.7 mm²/s Show Material materials with Difusividad térmica of 4.7 mm²/s | |
100.0 °C | 4.5 mm²/s Show Material materials with Difusividad térmica of 4.5 mm²/s | ||
200.0 °C | 4.6 mm²/s Show Material materials with Difusividad térmica of 4.6 mm²/s | ||
300.0 °C | 4.7 mm²/s Show Material materials with Difusividad térmica of 4.7 mm²/s | ||
400.0 °C | 4.5 mm²/s Show Material materials with Difusividad térmica of 4.5 mm²/s | ||
500.0 °C | 4.3 mm²/s Show Material materials with Difusividad térmica of 4.3 mm²/s | ||
600.0 °C | 3.7 mm²/s Show Material materials with Difusividad térmica of 3.7 mm²/s | ||
700.0 °C | 3 mm²/s Show Material materials with Difusividad térmica of 3 mm²/s | ||
Temperatura de fusión | 1370 - 1530 °C Show Material materials with Temperatura de fusión of 1370 - 1530 °C | Typical for Martensitic Stainless Steel | |
Temperatura máx. de funcionamiento, largo | -60 - 300 °C Show Material materials with Temperatura máx. de funcionamiento, largo of -60 - 300 °C |
Eléctrico
Property | Temperature | Value |
---|---|---|
Resistividad eléctrica | 20.0 °C | 6E-7 - 9.19E-7 Ω·m Show Material materials with Resistividad eléctrica of 6E-7 - 9.19E-7 Ω·m |
100.0 °C | 9.48E-7 Ω·m Show Material materials with Resistividad eléctrica of 9.48E-7 Ω·m | |
200.0 °C | 9.87E-7 Ω·m Show Material materials with Resistividad eléctrica of 9.87E-7 Ω·m | |
300.0 °C | 1.03E-6 Ω·m Show Material materials with Resistividad eléctrica of 1.03E-6 Ω·m | |
400.0 °C | 1.07E-6 Ω·m Show Material materials with Resistividad eléctrica of 1.07E-6 Ω·m | |
500.0 °C | 1.12E-6 Ω·m Show Material materials with Resistividad eléctrica of 1.12E-6 Ω·m | |
600.0 °C | 1.18E-6 Ω·m Show Material materials with Resistividad eléctrica of 1.18E-6 Ω·m | |
700.0 °C | 1.24E-6 Ω·m Show Material materials with Resistividad eléctrica of 1.24E-6 Ω·m | |
Chemical properties
Property | Value |
---|---|
Azufre | 0.015 % Show Material materials with Azufre of 0.015 % |
Carbono | 0.05 % Show Material materials with Carbono of 0.05 % |
Cromo | 12.5 - 14 % Show Material materials with Cromo of 12.5 - 14 % |
Fósforo | 0.04 % Show Material materials with Fósforo of 0.04 % |
Manganeso | 1 % Show Material materials with Manganeso of 1 % |
Molibdeno | 0.4 - 0.7 % Show Material materials with Molibdeno of 0.4 - 0.7 % |
Nitrógeno | 0.02 % Show Material materials with Nitrógeno of 0.02 % |
Níquel | 3.5 - 4.5 % Show Material materials with Níquel of 3.5 - 4.5 % |
Silicona | 0.6 % Show Material materials with Silicona of 0.6 % |