General
Property | Temperature | Value |
---|---|---|
Densidad | 20.0 °C | 7.7 - 7.73 g/cm³ Show Material materials with Densidad of 7.7 - 7.73 g/cm³ |
Mecánica
Property | Temperature | Value |
---|---|---|
Coeficiente de Poisson | 20.0 °C | 0.29 [-] Show Material materials with Coeficiente de Poisson of 0.29 [-] |
Dureza Brinell | 20.0 °C | 180 [-] Show Material materials with Dureza Brinell of 180 [-] |
Elongación | 20.0 °C | 24 % Show Material materials with Elongación of 24 % |
Límite elástico Rp 0,2 | 20.0 °C | 220 MPa Show Material materials with Límite elástico Rp 0,2 of 220 MPa |
50.0 °C | 215 MPa Show Material materials with Límite elástico Rp 0,2 of 215 MPa | |
100.0 °C | 195 MPa Show Material materials with Límite elástico Rp 0,2 of 195 MPa | |
150.0 °C | 180 MPa Show Material materials with Límite elástico Rp 0,2 of 180 MPa | |
200.0 °C | 170 MPa Show Material materials with Límite elástico Rp 0,2 of 170 MPa | |
250.0 °C | 160 MPa Show Material materials with Límite elástico Rp 0,2 of 160 MPa | |
300.0 °C | 155 MPa Show Material materials with Límite elástico Rp 0,2 of 155 MPa | |
Módulo de cizallamiento | 20.0 °C | 84.82 GPa Show Material materials with Módulo de cizallamiento of 84.82 GPa |
Módulo elástico | 20.0 °C | 217 - 220 GPa Show Material materials with Módulo elástico of 217 - 220 GPa |
100.0 °C | 215 - 216 GPa Show Material materials with Módulo elástico of 215 - 216 GPa | |
200.0 °C | 188 - 209 GPa Show Material materials with Módulo elástico of 188 - 209 GPa | |
300.0 °C | 164 - 200 GPa Show Material materials with Módulo elástico of 164 - 200 GPa | |
400.0 °C | 192 GPa Show Material materials with Módulo elástico of 192 GPa | |
500.0 °C | 183 GPa Show Material materials with Módulo elástico of 183 GPa | |
Resistencia a la tracción | 20.0 °C | 380 - 530 MPa Show Material materials with Resistencia a la tracción of 380 - 530 MPa |
Aplicaciones térmicas
Property | Temperature | Value | Comment |
---|---|---|---|
Calor específico | 20.0 °C | 430 - 439 J/(kg·K) Show Material materials with Calor específico of 430 - 439 J/(kg·K) | |
100.0 °C | 474 J/(kg·K) Show Material materials with Calor específico of 474 J/(kg·K) | ||
200.0 °C | 498 J/(kg·K) Show Material materials with Calor específico of 498 J/(kg·K) | ||
300.0 °C | 517 J/(kg·K) Show Material materials with Calor específico of 517 J/(kg·K) | ||
400.0 °C | 538 J/(kg·K) Show Material materials with Calor específico of 538 J/(kg·K) | ||
500.0 °C | 564 J/(kg·K) Show Material materials with Calor específico of 564 J/(kg·K) | ||
600.0 °C | 598 J/(kg·K) Show Material materials with Calor específico of 598 J/(kg·K) | ||
Coeficiente de dilatación térmica | 20.0 °C | 1.02E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.02E-5 1/K | |
100.0 °C | 1.04E-5 - 1.05E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.04E-5 - 1.05E-5 1/K | ||
200.0 °C | 1.08E-5 - 1.09E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.08E-5 - 1.09E-5 1/K | ||
300.0 °C | 1.12E-5 - 1.13E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.12E-5 - 1.13E-5 1/K | ||
400.0 °C | 1.16E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.16E-5 1/K | ||
500.0 °C | 1.19E-5 - 1.2E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.19E-5 - 1.2E-5 1/K | ||
600.0 °C | 1.22E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.22E-5 1/K | ||
Conductividad térmica | 20.0 °C | 20 - 25.9 W/(m·K) Show Material materials with Conductividad térmica of 20 - 25.9 W/(m·K) | |
100.0 °C | 25.3 W/(m·K) Show Material materials with Conductividad térmica of 25.3 W/(m·K) | ||
200.0 °C | 25.2 W/(m·K) Show Material materials with Conductividad térmica of 25.2 W/(m·K) | ||
300.0 °C | 25.2 W/(m·K) Show Material materials with Conductividad térmica of 25.2 W/(m·K) | ||
400.0 °C | 25.4 W/(m·K) Show Material materials with Conductividad térmica of 25.4 W/(m·K) | ||
500.0 °C | 25.7 W/(m·K) Show Material materials with Conductividad térmica of 25.7 W/(m·K) | ||
600.0 °C | 25.9 W/(m·K) Show Material materials with Conductividad térmica of 25.9 W/(m·K) | ||
Difusividad térmica | 20.0 °C | 7.6 mm²/s Show Material materials with Difusividad térmica of 7.6 mm²/s | |
100.0 °C | 6.6 mm²/s Show Material materials with Difusividad térmica of 6.6 mm²/s | ||
200.0 °C | 6.1 mm²/s Show Material materials with Difusividad térmica of 6.1 mm²/s | ||
300.0 °C | 5.8 mm²/s Show Material materials with Difusividad térmica of 5.8 mm²/s | ||
400.0 °C | 5.3 mm²/s Show Material materials with Difusividad térmica of 5.3 mm²/s | ||
500.0 °C | 4.8 mm²/s Show Material materials with Difusividad térmica of 4.8 mm²/s | ||
600.0 °C | 4.1 mm²/s Show Material materials with Difusividad térmica of 4.1 mm²/s | ||
Temperatura de fusión | 1425 - 1530 °C Show Material materials with Temperatura de fusión of 1425 - 1530 °C | Typical for Ferritic Stainless Steel |
Eléctrico
Property | Temperature | Value |
---|---|---|
Resistividad eléctrica | 20.0 °C | 5.59E-7 - 7E-7 Ω·m Show Material materials with Resistividad eléctrica of 5.59E-7 - 7E-7 Ω·m |
100.0 °C | 6.4E-7 Ω·m Show Material materials with Resistividad eléctrica of 6.4E-7 Ω·m | |
200.0 °C | 7.32E-7 Ω·m Show Material materials with Resistividad eléctrica of 7.32E-7 Ω·m | |
300.0 °C | 8.17E-7 Ω·m Show Material materials with Resistividad eléctrica of 8.17E-7 Ω·m | |
400.0 °C | 8.97E-7 Ω·m Show Material materials with Resistividad eléctrica of 8.97E-7 Ω·m | |
500.0 °C | 9.74E-7 Ω·m Show Material materials with Resistividad eléctrica of 9.74E-7 Ω·m | |
600.0 °C | 1.05E-6 Ω·m Show Material materials with Resistividad eléctrica of 1.05E-6 Ω·m | |
Chemical properties
Property | Value |
---|---|
Azufre | 0.02 % Show Material materials with Azufre of 0.02 % |
Carbono | 0.015 % Show Material materials with Carbono of 0.015 % |
Cromo | 14 - 16 % Show Material materials with Cromo of 14 - 16 % |
Fósforo | 0.03 % Show Material materials with Fósforo of 0.03 % |
Manganeso | 0.5 % Show Material materials with Manganeso of 0.5 % |
Nitrógeno | 0.02 % Show Material materials with Nitrógeno of 0.02 % |
Silicona | 0.5 % Show Material materials with Silicona of 0.5 % |
Titanio | 0.25 - 0.4 % Show Material materials with Titanio of 0.25 - 0.4 % |