General
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Densidad | 20 °C | 7.84 g/cm³ Show Material materials with Densidad of 7.84 g/cm³ | thermomechanically rolled | EN 10149-2 | Flat |
Mecánica
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Coeficiente de Poisson | 0.29 [-] Show Material materials with Coeficiente de Poisson of 0.29 [-] | Typical for Low Carbon Steel | ||||
Dureza Brinell | 243 [-] Show Material materials with Dureza Brinell of 243 [-] | Predicted Value, Transverse | ||||
Elongación | 14.5 % Show Material materials with Elongación of 14.5 % | Predicted Value, A200 | ||||
16.5 % Show Material materials with Elongación of 16.5 % | Predicted Value, Transverse | |||||
17.1 % Show Material materials with Elongación of 17.1 % | Predicted Value, A80 Transverse | |||||
18.7 % Show Material materials with Elongación of 18.7 % | Predicted Value, A50 | |||||
21.2 % Show Material materials with Elongación of 21.2 % | Predicted Value, A5 | |||||
20 °C | 14 % Show Material materials with Elongación of 14 % | thermomechanically rolled | EN 10149-2 | Flat | A80 | |
20 °C | 17 % Show Material materials with Elongación of 17 % | thermomechanically rolled | EN 10149-2 | Flat | ||
Estricción | 39.3 % Show Material materials with Estricción of 39.3 % | Predicted Value | ||||
44.1 % Show Material materials with Estricción of 44.1 % | Predicted Value, Transverse | |||||
Límite elástico | 252.3 MPa Show Material materials with Límite elástico of 252.3 MPa | Predicted Value, RP1 | ||||
298.7 MPa Show Material materials with Límite elástico of 298.7 MPa | Predicted Value, RP1 Transverse | |||||
399.3 MPa Show Material materials with Límite elástico of 399.3 MPa | Predicted Value, Transverse | |||||
451.1 MPa Show Material materials with Límite elástico of 451.1 MPa | Predicted Value, RP02 | |||||
466 MPa Show Material materials with Límite elástico of 466 MPa | Predicted Value, RP05 | |||||
481.6 MPa Show Material materials with Límite elástico of 481.6 MPa | Predicted Value, RP02 Transverse | |||||
516.2 MPa Show Material materials with Límite elástico of 516.2 MPa | Predicted Value, RP002 | |||||
20 °C | 460 MPa Show Material materials with Límite elástico of 460 MPa | thermomechanically rolled | EN 10149-2 | Flat | ||
Módulo de cizallamiento | 82 GPa Show Material materials with Módulo de cizallamiento of 82 GPa | Typical for Low Carbon Steel | ||||
Módulo elástico | -100 °C | 217 GPa Show Material materials with Módulo elástico of 217 GPa | thermomechanically rolled | EN 10149-2 | Flat | |
20 °C | 212 GPa Show Material materials with Módulo elástico of 212 GPa | thermomechanically rolled | EN 10149-2 | Flat | ||
100 °C | 207 GPa Show Material materials with Módulo elástico of 207 GPa | thermomechanically rolled | EN 10149-2 | Flat | ||
200 °C | 199 GPa Show Material materials with Módulo elástico of 199 GPa | thermomechanically rolled | EN 10149-2 | Flat | ||
300 °C | 192 GPa Show Material materials with Módulo elástico of 192 GPa | thermomechanically rolled | EN 10149-2 | Flat | ||
400 °C | 184 GPa Show Material materials with Módulo elástico of 184 GPa | thermomechanically rolled | EN 10149-2 | Flat | ||
500 °C | 175 GPa Show Material materials with Módulo elástico of 175 GPa | thermomechanically rolled | EN 10149-2 | Flat | ||
600 °C | 164 GPa Show Material materials with Módulo elástico of 164 GPa | thermomechanically rolled | EN 10149-2 | Flat | ||
Resistencia a la tracción | 20 °C | 520 - 670 MPa Show Material materials with Resistencia a la tracción of 520 - 670 MPa | thermomechanically rolled | EN 10149-2 | Flat | |
Resistencia al cizallamiento | 500.8 MPa Show Material materials with Resistencia al cizallamiento of 500.8 MPa | Predicted Value |
Aplicaciones térmicas
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Calor específico | -100 °C | 423 J/(kg·K) Show Material materials with Calor específico of 423 J/(kg·K) | thermomechanically rolled | EN 10149-2 | Flat | |
20 °C | 461 J/(kg·K) Show Material materials with Calor específico of 461 J/(kg·K) | thermomechanically rolled | EN 10149-2 | Flat | ||
100 °C | 479 J/(kg·K) Show Material materials with Calor específico of 479 J/(kg·K) | thermomechanically rolled | EN 10149-2 | Flat | ||
200 °C | 499 J/(kg·K) Show Material materials with Calor específico of 499 J/(kg·K) | thermomechanically rolled | EN 10149-2 | Flat | ||
300 °C | 517 J/(kg·K) Show Material materials with Calor específico of 517 J/(kg·K) | thermomechanically rolled | EN 10149-2 | Flat | ||
400 °C | 536 J/(kg·K) Show Material materials with Calor específico of 536 J/(kg·K) | thermomechanically rolled | EN 10149-2 | Flat | ||
500 °C | 558 J/(kg·K) Show Material materials with Calor específico of 558 J/(kg·K) | thermomechanically rolled | EN 10149-2 | Flat | ||
600 °C | 587 J/(kg·K) Show Material materials with Calor específico of 587 J/(kg·K) | thermomechanically rolled | EN 10149-2 | Flat | ||
Coeficiente de dilatación térmica | -100 °C | 1.08e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 1.08e-05 1/K | thermomechanically rolled | EN 10149-2 | Flat | |
20 °C | 1.19e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 1.19e-05 1/K | thermomechanically rolled | EN 10149-2 | Flat | ||
100 °C | 1.25e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 1.25e-05 1/K | thermomechanically rolled | EN 10149-2 | Flat | ||
200 °C | 1.3e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 1.3e-05 1/K | thermomechanically rolled | EN 10149-2 | Flat | ||
300 °C | 1.36e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 1.36e-05 1/K | thermomechanically rolled | EN 10149-2 | Flat | ||
400 °C | 1.41e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 1.41e-05 1/K | thermomechanically rolled | EN 10149-2 | Flat | ||
500 °C | 1.45e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 1.45e-05 1/K | thermomechanically rolled | EN 10149-2 | Flat | ||
600 °C | 1.49e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 1.49e-05 1/K | thermomechanically rolled | EN 10149-2 | Flat | ||
Conductividad térmica | -100 °C | 46.5 W/(m·K) Show Material materials with Conductividad térmica of 46.5 W/(m·K) | thermomechanically rolled | EN 10149-2 | Flat | |
20 °C | 49.4 W/(m·K) Show Material materials with Conductividad térmica of 49.4 W/(m·K) | thermomechanically rolled | EN 10149-2 | Flat | ||
100 °C | 49.4 W/(m·K) Show Material materials with Conductividad térmica of 49.4 W/(m·K) | thermomechanically rolled | EN 10149-2 | Flat | ||
200 °C | 47.8 W/(m·K) Show Material materials with Conductividad térmica of 47.8 W/(m·K) | thermomechanically rolled | EN 10149-2 | Flat | ||
300 °C | 45.1 W/(m·K) Show Material materials with Conductividad térmica of 45.1 W/(m·K) | thermomechanically rolled | EN 10149-2 | Flat | ||
400 °C | 41.8 W/(m·K) Show Material materials with Conductividad térmica of 41.8 W/(m·K) | thermomechanically rolled | EN 10149-2 | Flat | ||
500 °C | 38.6 W/(m·K) Show Material materials with Conductividad térmica of 38.6 W/(m·K) | thermomechanically rolled | EN 10149-2 | Flat | ||
600 °C | 35.3 W/(m·K) Show Material materials with Conductividad térmica of 35.3 W/(m·K) | thermomechanically rolled | EN 10149-2 | Flat | ||
Difusividad térmica | -100 °C | 15.9 mm²/s Show Material materials with Difusividad térmica of 15.9 mm²/s | thermomechanically rolled | EN 10149-2 | Flat | |
20 °C | 13.7 mm²/s Show Material materials with Difusividad térmica of 13.7 mm²/s | thermomechanically rolled | EN 10149-2 | Flat | ||
100 °C | 12.7 mm²/s Show Material materials with Difusividad térmica of 12.7 mm²/s | thermomechanically rolled | EN 10149-2 | Flat | ||
200 °C | 11.5 mm²/s Show Material materials with Difusividad térmica of 11.5 mm²/s | thermomechanically rolled | EN 10149-2 | Flat | ||
300 °C | 10.2 mm²/s Show Material materials with Difusividad térmica of 10.2 mm²/s | thermomechanically rolled | EN 10149-2 | Flat | ||
400 °C | 8.9 mm²/s Show Material materials with Difusividad térmica of 8.9 mm²/s | thermomechanically rolled | EN 10149-2 | Flat | ||
500 °C | 7.4 mm²/s Show Material materials with Difusividad térmica of 7.4 mm²/s | thermomechanically rolled | EN 10149-2 | Flat | ||
600 °C | 5.8 mm²/s Show Material materials with Difusividad térmica of 5.8 mm²/s | thermomechanically rolled | EN 10149-2 | Flat | ||
Temperatura de fusión | 1480 - 1526 °C Show Material materials with Temperatura de fusión of 1480 - 1526 °C | Typical for Low Carbon Steel | ||||
Temperatura máx. de funcionamiento | -20 °C Show Material materials with Temperatura máx. de funcionamiento of -20 °C | thermomechanically rolled | EN 10149-2 | Flat | Long | |
500 °C Show Material materials with Temperatura máx. de funcionamiento of 500 °C | Typical for Carbon Steel |
Eléctrico
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Conductividad eléctrica | 7 S/m Show Material materials with Conductividad eléctrica of 7 S/m | Predicted Value | ||||
Resistividad eléctrica | -100 °C | 1.47e-07 Ω·m Show Material materials with Resistividad eléctrica of 1.47e-07 Ω·m | thermomechanically rolled | EN 10149-2 | Flat | |
20 °C | 2.11e-07 Ω·m Show Material materials with Resistividad eléctrica of 2.11e-07 Ω·m | thermomechanically rolled | EN 10149-2 | Flat | ||
100 °C | 2.59e-07 Ω·m Show Material materials with Resistividad eléctrica of 2.59e-07 Ω·m | thermomechanically rolled | EN 10149-2 | Flat | ||
200 °C | 3.3e-07 Ω·m Show Material materials with Resistividad eléctrica of 3.3e-07 Ω·m | thermomechanically rolled | EN 10149-2 | Flat | ||
300 °C | 4.16e-07 Ω·m Show Material materials with Resistividad eléctrica of 4.16e-07 Ω·m | thermomechanically rolled | EN 10149-2 | Flat | ||
400 °C | 5.2e-07 Ω·m Show Material materials with Resistividad eléctrica of 5.2e-07 Ω·m | thermomechanically rolled | EN 10149-2 | Flat | ||
500 °C | 6.41e-07 Ω·m Show Material materials with Resistividad eléctrica of 6.41e-07 Ω·m | thermomechanically rolled | EN 10149-2 | Flat | ||
600 °C | 7.85e-07 Ω·m Show Material materials with Resistividad eléctrica of 7.85e-07 Ω·m | thermomechanically rolled | EN 10149-2 | Flat |
Magnético
Property | Value | Comment |
---|---|---|
Temperatura de Curie | 770 °C Show Material materials with Temperatura de Curie of 770 °C | Typical for Low Carbon Steel |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Aluminio | 0.015 % Show Material materials with Aluminio of 0.015 % | thermomechanically rolled | EN 10149-2 | Flat |
Azufre | 0.015 % Show Material materials with Azufre of 0.015 % | thermomechanically rolled | EN 10149-2 | Flat |
Carbono | 0.12 % Show Material materials with Carbono of 0.12 % | thermomechanically rolled | EN 10149-2 | Flat |
Fósforo | 0.025 % Show Material materials with Fósforo of 0.025 % | thermomechanically rolled | EN 10149-2 | Flat |
Manganeso | 1.6 % Show Material materials with Manganeso of 1.6 % | thermomechanically rolled | EN 10149-2 | Flat |
Niobio | 0.09 % Show Material materials with Niobio of 0.09 % | thermomechanically rolled | EN 10149-2 | Flat |
Silicona | 0.5 % Show Material materials with Silicona of 0.5 % | thermomechanically rolled | EN 10149-2 | Flat |
Titanio | 0.15 % Show Material materials with Titanio of 0.15 % | thermomechanically rolled | EN 10149-2 | Flat |
Vanadio | 0.2 % Show Material materials with Vanadio of 0.2 % | thermomechanically rolled | EN 10149-2 | Flat |