General
Property | Temperature | Value | Condition | Related Standards |
---|---|---|---|---|
Densidad | 20.0 °C | 2.68 g/cm³ Show Material materials with Densidad of 2.68 g/cm³ | G25 | DIN 1725-1, EN 573-3, EN 573-4, WL 3.3524-1 |
Mecánica
Property | Temperature | Value | Condition | Related Standards | Comment |
---|---|---|---|---|---|
Coeficiente de Poisson | 0.33 [-] Show Material materials with Coeficiente de Poisson of 0.33 [-] | Typical for Wrought 5000 Series Aluminium | |||
Elongación | -196.0 °C | 28.0 % Show Material materials with Elongación of 28.0 % | G25 | DIN 1725-1, EN 573-3, EN 573-4, WL 3.3524-1 | |
-80.0 °C | 21.0 % Show Material materials with Elongación of 21.0 % | G25 | DIN 1725-1, EN 573-3, EN 573-4, WL 3.3524-1 | ||
-28.0 °C | 18.0 % Show Material materials with Elongación of 18.0 % | G25 | DIN 1725-1, EN 573-3, EN 573-4, WL 3.3524-1 | ||
20.0 °C | 16.0 % Show Material materials with Elongación of 16.0 % | G25 | DIN 1725-1, EN 573-3, EN 573-4, WL 3.3524-1 | ||
100.0 °C | 18.0 % Show Material materials with Elongación of 18.0 % | G25 | DIN 1725-1, EN 573-3, EN 573-4, WL 3.3524-1 | ||
150.0 °C | 27.0 % Show Material materials with Elongación of 27.0 % | G25 | DIN 1725-1, EN 573-3, EN 573-4, WL 3.3524-1 | ||
200.0 °C | 45.0 % Show Material materials with Elongación of 45.0 % | G25 | DIN 1725-1, EN 573-3, EN 573-4, WL 3.3524-1 | ||
260.0 °C | 80.0 % Show Material materials with Elongación of 80.0 % | G25 | DIN 1725-1, EN 573-3, EN 573-4, WL 3.3524-1 | ||
315.0 °C | 110.0 % Show Material materials with Elongación of 110.0 % | G25 | DIN 1725-1, EN 573-3, EN 573-4, WL 3.3524-1 | ||
370.0 °C | 130.0 % Show Material materials with Elongación of 130.0 % | G25 | DIN 1725-1, EN 573-3, EN 573-4, WL 3.3524-1 | ||
Módulo de cizallamiento | 20.0 °C | 27.0 Show Material materials with Módulo de cizallamiento of 27.0 | G25 | DIN 1725-1, EN 573-3, EN 573-4, WL 3.3524-1 | |
Módulo elástico | 20.0 °C | 72.0 Show Material materials with Módulo elástico of 72.0 | G25 | DIN 1725-1, EN 573-3, EN 573-4, WL 3.3524-1 | |
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 5000 Series Aluminium | |||
Resistencia a la tracción | -196.0 °C | 380.0 MPa Show Material materials with Resistencia a la tracción of 380.0 MPa | G25 | DIN 1725-1, EN 573-3, EN 573-4, WL 3.3524-1 | |
-80.0 °C | 280.0 MPa Show Material materials with Resistencia a la tracción of 280.0 MPa | G25 | DIN 1725-1, EN 573-3, EN 573-4, WL 3.3524-1 | ||
-28.0 °C | 260.0 MPa Show Material materials with Resistencia a la tracción of 260.0 MPa | G25 | DIN 1725-1, EN 573-3, EN 573-4, WL 3.3524-1 | ||
20.0 °C | 260.0 MPa Show Material materials with Resistencia a la tracción of 260.0 MPa | G25 | DIN 1725-1, EN 573-3, EN 573-4, WL 3.3524-1 | ||
100.0 °C | 260.0 MPa Show Material materials with Resistencia a la tracción of 260.0 MPa | G25 | DIN 1725-1, EN 573-3, EN 573-4, WL 3.3524-1 | ||
150.0 °C | 205.0 MPa Show Material materials with Resistencia a la tracción of 205.0 MPa | G25 | DIN 1725-1, EN 573-3, EN 573-4, WL 3.3524-1 | ||
200.0 °C | 165.0 MPa Show Material materials with Resistencia a la tracción of 165.0 MPa | G25 | DIN 1725-1, EN 573-3, EN 573-4, WL 3.3524-1 | ||
260.0 °C | 85.0 MPa Show Material materials with Resistencia a la tracción of 85.0 MPa | G25 | DIN 1725-1, EN 573-3, EN 573-4, WL 3.3524-1 | ||
315.0 °C | 50.0 MPa Show Material materials with Resistencia a la tracción of 50.0 MPa | G25 | DIN 1725-1, EN 573-3, EN 573-4, WL 3.3524-1 | ||
370.0 °C | 35.0 MPa Show Material materials with Resistencia a la tracción of 35.0 MPa | G25 | DIN 1725-1, EN 573-3, EN 573-4, WL 3.3524-1 |
Aplicaciones térmicas
Property | Temperature | Value | Condition | Related Standards | Comment |
---|---|---|---|---|---|
Calor específico | 20.0 °C | 900.0 J/(kg·K) Show Material materials with Calor específico of 900.0 J/(kg·K) | G25 | DIN 1725-1, EN 573-3, EN 573-4, WL 3.3524-1 | |
Coeficiente de dilatación térmica | -50.0 °C | 2.21e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.21e-05 1/K | G25 | DIN 1725-1, EN 573-3, EN 573-4, WL 3.3524-1 | |
100.0 °C | 2.38e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.38e-05 1/K | G25 | DIN 1725-1, EN 573-3, EN 573-4, WL 3.3524-1 | ||
200.0 °C | 2.48e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.48e-05 1/K | G25 | DIN 1725-1, EN 573-3, EN 573-4, WL 3.3524-1 | ||
300.0 °C | 2.57e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.57e-05 1/K | G25 | DIN 1725-1, EN 573-3, EN 573-4, WL 3.3524-1 | ||
Conductividad térmica | 20.0 °C | 150.0 Show Material materials with Conductividad térmica of 150.0 | G25 | DIN 1725-1, EN 573-3, EN 573-4, WL 3.3524-1 | |
Temperatura de fusión | 560.0 - 655.0 °C Show Material materials with Temperatura de fusión of 560.0 - 655.0 °C | Typical for Wrought 5000 Series Aluminium | |||
Temperatura máx. de funcionamiento | 150.0 °C Show Material materials with Temperatura máx. de funcionamiento of 150.0 °C | Typical for Wrought 5000 Series Aluminium |
Eléctrico
Property | Temperature | Value | Condition | Related Standards | Comment |
---|---|---|---|---|---|
Conductividad eléctrica | 20.0 °C | 21000000.0 Show Material materials with Conductividad eléctrica of 21000000.0 | G25 | DIN 1725-1, EN 573-3, EN 573-4, WL 3.3524-1 | |
Resistividad eléctrica | 3.3e-08 - 5e-08 Ω·m Show Material materials with Resistividad eléctrica of 3.3e-08 - 5e-08 Ω·m | Typical for Wrought 5000 Series Aluminium |
Chemical properties
Property | Value | Condition | Related Standards |
---|---|---|---|
Cobre | 0.1 Show Material materials with Cobre of 0.1 | G25 | DIN 1725-1, EN 573-3, EN 573-4, WL 3.3524-1 |
Cromo | 0.15 - 0.35 % Show Material materials with Cromo of 0.15 - 0.35 % | G25 | DIN 1725-1, EN 573-3, EN 573-4, WL 3.3524-1 |
Hierro | 0.4 Show Material materials with Hierro of 0.4 | G25 | DIN 1725-1, EN 573-3, EN 573-4, WL 3.3524-1 |
Magnesio | 2.2 - 2.8 % Show Material materials with Magnesio of 2.2 - 2.8 % | G25 | DIN 1725-1, EN 573-3, EN 573-4, WL 3.3524-1 |
Manganeso | 0.1 Show Material materials with Manganeso of 0.1 | G25 | DIN 1725-1, EN 573-3, EN 573-4, WL 3.3524-1 |
Silicona | 0.25 Show Material materials with Silicona of 0.25 | G25 | DIN 1725-1, EN 573-3, EN 573-4, WL 3.3524-1 |
Zinc | 0.1 Show Material materials with Zinc of 0.1 | G25 | DIN 1725-1, EN 573-3, EN 573-4, WL 3.3524-1 |
Technological properties
Property | ||
---|---|---|
Workability | Good workability. |