General
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Densidad | 20 °C | 7.85 g/cm³ Show Material materials with Densidad of 7.85 g/cm³ | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire |
Mecánica
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Coeficiente de Poisson | 20 °C | 0.284 [-] Show Material materials with Coeficiente de Poisson of 0.284 [-] | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | |
Dureza Brinell | 246 [-] Show Material materials with Dureza Brinell of 246 [-] | Predicted Value, Transverse | ||||
Elongación | 17.8 % Show Material materials with Elongación of 17.8 % | Predicted Value, A200 | ||||
21.5 % Show Material materials with Elongación of 21.5 % | Predicted Value, A5 | |||||
23.8 % Show Material materials with Elongación of 23.8 % | Predicted Value, A50 | |||||
20 °C | 13 % Show Material materials with Elongación of 13 % | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | A80 Transverse | |
20 °C | 14 % Show Material materials with Elongación of 14 % | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | A80 Transverse | |
20 °C | 15 % Show Material materials with Elongación of 15 % | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | A80 Transverse | |
20 °C | 15 % Show Material materials with Elongación of 15 % | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | A80 | |
20 °C | 16 % Show Material materials with Elongación of 16 % | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | A80 Transverse | |
20 °C | 16 % Show Material materials with Elongación of 16 % | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | A80 | |
20 °C | 17 % Show Material materials with Elongación of 17 % | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | A80 Transverse | |
20 °C | 17 % Show Material materials with Elongación of 17 % | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | A80 | |
20 °C | 18 % Show Material materials with Elongación of 18 % | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | A80 | |
20 °C | 18 % Show Material materials with Elongación of 18 % | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | Transverse | |
20 °C | 18 % Show Material materials with Elongación of 18 % | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 19 % Show Material materials with Elongación of 19 % | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | A80 | |
20 °C | 19 % Show Material materials with Elongación of 19 % | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | Transverse | |
20 °C | 19 % Show Material materials with Elongación of 19 % | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 20 % Show Material materials with Elongación of 20 % | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | Transverse | |
20 °C | 21 % Show Material materials with Elongación of 21 % | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | Transverse | |
20 °C | 21 % Show Material materials with Elongación of 21 % | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 22 % Show Material materials with Elongación of 22 % | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 23 % Show Material materials with Elongación of 23 % | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
Estricción | 43.7 % Show Material materials with Estricción of 43.7 % | Predicted Value, Transverse | ||||
50.5 % Show Material materials with Estricción of 50.5 % | Predicted Value | |||||
Límite elástico | 248.3 MPa Show Material materials with Límite elástico of 248.3 MPa | Predicted Value, RP1 | ||||
307.7 MPa Show Material materials with Límite elástico of 307.7 MPa | Predicted Value, Transverse | |||||
311.8 MPa Show Material materials with Límite elástico of 311.8 MPa | Predicted Value, RP1 Transverse | |||||
334.3 MPa Show Material materials with Límite elástico of 334.3 MPa | Predicted Value, RP05 | |||||
348.8 MPa Show Material materials with Límite elástico of 348.8 MPa | Predicted Value, RP02 | |||||
454.2 MPa Show Material materials with Límite elástico of 454.2 MPa | Predicted Value, RP02 Transverse | |||||
470 MPa Show Material materials with Límite elástico of 470 MPa | Predicted Value, RP002 | |||||
20 °C | 205 MPa Show Material materials with Límite elástico of 205 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 215 MPa Show Material materials with Límite elástico of 215 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 225 MPa Show Material materials with Límite elástico of 225 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 235 MPa Show Material materials with Límite elástico of 235 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 245 MPa Show Material materials with Límite elástico of 245 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 255 MPa Show Material materials with Límite elástico of 255 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 265 MPa Show Material materials with Límite elástico of 265 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 275 MPa Show Material materials with Límite elástico of 275 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
100 °C | 180 - 220 MPa Show Material materials with Límite elástico of 180 - 220 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
100 °C | 180 - 210 MPa Show Material materials with Límite elástico of 180 - 210 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
100 °C | 180 - 188 MPa Show Material materials with Límite elástico of 180 - 188 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
100 °C | 180 MPa Show Material materials with Límite elástico of 180 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
100 °C | 188 - 220 MPa Show Material materials with Límite elástico of 188 - 220 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
100 °C | 188 - 210 MPa Show Material materials with Límite elástico of 188 - 210 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
100 °C | 188 MPa Show Material materials with Límite elástico of 188 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
100 °C | 210 - 220 MPa Show Material materials with Límite elástico of 210 - 220 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
100 °C | 210 MPa Show Material materials with Límite elástico of 210 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
100 °C | 220 MPa Show Material materials with Límite elástico of 220 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
200 °C | 155 - 190 MPa Show Material materials with Límite elástico of 155 - 190 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
200 °C | 155 - 180 MPa Show Material materials with Límite elástico of 155 - 180 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
200 °C | 155 - 162 MPa Show Material materials with Límite elástico of 155 - 162 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
200 °C | 155 MPa Show Material materials with Límite elástico of 155 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
200 °C | 162 - 190 MPa Show Material materials with Límite elástico of 162 - 190 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
200 °C | 162 - 180 MPa Show Material materials with Límite elástico of 162 - 180 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
200 °C | 162 MPa Show Material materials with Límite elástico of 162 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
200 °C | 180 MPa Show Material materials with Límite elástico of 180 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
200 °C | 180 - 190 MPa Show Material materials with Límite elástico of 180 - 190 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
200 °C | 190 MPa Show Material materials with Límite elástico of 190 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
250 °C | 144 - 180 MPa Show Material materials with Límite elástico of 144 - 180 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
250 °C | 144 - 170 MPa Show Material materials with Límite elástico of 144 - 170 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
250 °C | 144 - 150 MPa Show Material materials with Límite elástico of 144 - 150 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
250 °C | 144 MPa Show Material materials with Límite elástico of 144 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
250 °C | 150 - 180 MPa Show Material materials with Límite elástico of 150 - 180 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
250 °C | 150 - 170 MPa Show Material materials with Límite elástico of 150 - 170 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
250 °C | 150 MPa Show Material materials with Límite elástico of 150 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
250 °C | 170 - 180 MPa Show Material materials with Límite elástico of 170 - 180 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
250 °C | 170 MPa Show Material materials with Límite elástico of 170 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
250 °C | 180 MPa Show Material materials with Límite elástico of 180 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
300 °C | 119 - 150 MPa Show Material materials with Límite elástico of 119 - 150 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
300 °C | 119 - 140 MPa Show Material materials with Límite elástico of 119 - 140 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
300 °C | 119 - 124 MPa Show Material materials with Límite elástico of 119 - 124 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
300 °C | 119 MPa Show Material materials with Límite elástico of 119 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
300 °C | 124 - 150 MPa Show Material materials with Límite elástico of 124 - 150 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
300 °C | 124 - 140 MPa Show Material materials with Límite elástico of 124 - 140 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
300 °C | 124 MPa Show Material materials with Límite elástico of 124 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
300 °C | 140 - 150 MPa Show Material materials with Límite elástico of 140 - 150 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
300 °C | 140 MPa Show Material materials with Límite elástico of 140 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
300 °C | 150 MPa Show Material materials with Límite elástico of 150 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | |||
Módulo de cizallamiento | 82 GPa Show Material materials with Módulo de cizallamiento of 82 GPa | Typical for Low Carbon Steel | ||||
Módulo elástico | -100 °C | 217 GPa Show Material materials with Módulo elástico of 217 GPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | |
20 °C | 212 GPa Show Material materials with Módulo elástico of 212 GPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
100 °C | 207 GPa Show Material materials with Módulo elástico of 207 GPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
200 °C | 199 GPa Show Material materials with Módulo elástico of 199 GPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
300 °C | 192 GPa Show Material materials with Módulo elástico of 192 GPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
400 °C | 184 GPa Show Material materials with Módulo elástico of 184 GPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
500 °C | 175 GPa Show Material materials with Módulo elástico of 175 GPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
600 °C | 164 GPa Show Material materials with Módulo elástico of 164 GPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
Resistencia a la tracción | 20 °C | 380 - 580 MPa Show Material materials with Resistencia a la tracción of 380 - 580 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | |
20 °C | 380 - 560 MPa Show Material materials with Resistencia a la tracción of 380 - 560 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 380 - 540 MPa Show Material materials with Resistencia a la tracción of 380 - 540 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 400 - 580 MPa Show Material materials with Resistencia a la tracción of 400 - 580 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 400 - 560 MPa Show Material materials with Resistencia a la tracción of 400 - 560 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 400 - 540 MPa Show Material materials with Resistencia a la tracción of 400 - 540 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 410 - 580 MPa Show Material materials with Resistencia a la tracción of 410 - 580 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 410 - 560 MPa Show Material materials with Resistencia a la tracción of 410 - 560 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 410 - 540 MPa Show Material materials with Resistencia a la tracción of 410 - 540 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 430 - 580 MPa Show Material materials with Resistencia a la tracción of 430 - 580 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 430 - 560 MPa Show Material materials with Resistencia a la tracción of 430 - 560 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 430 - 540 MPa Show Material materials with Resistencia a la tracción of 430 - 540 MPa | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
Resistencia al cizallamiento | 487.6 MPa Show Material materials with Resistencia al cizallamiento of 487.6 MPa | Predicted Value |
Aplicaciones térmicas
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Calor específico | -100 °C | 423 J/(kg·K) Show Material materials with Calor específico of 423 J/(kg·K) | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | |
20 °C | 461 J/(kg·K) Show Material materials with Calor específico of 461 J/(kg·K) | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
100 °C | 479 J/(kg·K) Show Material materials with Calor específico of 479 J/(kg·K) | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
200 °C | 499 J/(kg·K) Show Material materials with Calor específico of 499 J/(kg·K) | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
300 °C | 517 J/(kg·K) Show Material materials with Calor específico of 517 J/(kg·K) | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
400 °C | 536 J/(kg·K) Show Material materials with Calor específico of 536 J/(kg·K) | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
500 °C | 558 J/(kg·K) Show Material materials with Calor específico of 558 J/(kg·K) | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
600 °C | 587 J/(kg·K) Show Material materials with Calor específico of 587 J/(kg·K) | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
Coeficiente de dilatación térmica | -100 °C | 1.08e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 1.08e-05 1/K | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | |
20 °C | 1.19e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 1.19e-05 1/K | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
100 °C | 1.25e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 1.25e-05 1/K | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
200 °C | 1.3e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 1.3e-05 1/K | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
300 °C | 1.36e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 1.36e-05 1/K | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
400 °C | 1.41e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 1.41e-05 1/K | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
500 °C | 1.45e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 1.45e-05 1/K | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
600 °C | 1.49e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 1.49e-05 1/K | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
Conductividad térmica | 20 °C | 53.4 W/(m·K) Show Material materials with Conductividad térmica of 53.4 W/(m·K) | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | |
100 °C | 52.9 W/(m·K) Show Material materials with Conductividad térmica of 52.9 W/(m·K) | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
200 °C | 50.3 W/(m·K) Show Material materials with Conductividad térmica of 50.3 W/(m·K) | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
300 °C | 46.7 W/(m·K) Show Material materials with Conductividad térmica of 46.7 W/(m·K) | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
400 °C | 43.3 W/(m·K) Show Material materials with Conductividad térmica of 43.3 W/(m·K) | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
500 °C | 39.8 W/(m·K) Show Material materials with Conductividad térmica of 39.8 W/(m·K) | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
600 °C | 36.7 W/(m·K) Show Material materials with Conductividad térmica of 36.7 W/(m·K) | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
Difusividad térmica | 20 °C | 14.8 mm²/s Show Material materials with Difusividad térmica of 14.8 mm²/s | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | |
100 °C | 13.6 mm²/s Show Material materials with Difusividad térmica of 13.6 mm²/s | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
200 °C | 12.1 mm²/s Show Material materials with Difusividad térmica of 12.1 mm²/s | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
300 °C | 10.6 mm²/s Show Material materials with Difusividad térmica of 10.6 mm²/s | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
400 °C | 9.2 mm²/s Show Material materials with Difusividad térmica of 9.2 mm²/s | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
500 °C | 7.7 mm²/s Show Material materials with Difusividad térmica of 7.7 mm²/s | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
600 °C | 6.2 mm²/s Show Material materials with Difusividad térmica of 6.2 mm²/s | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
Temperatura de fusión | 1480 - 1526 °C Show Material materials with Temperatura de fusión of 1480 - 1526 °C | Typical for Low Carbon Steel | ||||
Temperatura máx. de funcionamiento | 336.1 °C Show Material materials with Temperatura máx. de funcionamiento of 336.1 °C | Predicted Value, Long | ||||
500 °C Show Material materials with Temperatura máx. de funcionamiento of 500 °C | Typical for Carbon Steel |
Eléctrico
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Conductividad eléctrica | 8 S/m Show Material materials with Conductividad eléctrica of 8 S/m | Predicted Value | ||||
Resistividad eléctrica | 20 °C | 1.95e-07 Ω·m Show Material materials with Resistividad eléctrica of 1.95e-07 Ω·m | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | |
100 °C | 2.42e-07 Ω·m Show Material materials with Resistividad eléctrica of 2.42e-07 Ω·m | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
200 °C | 3.14e-07 Ω·m Show Material materials with Resistividad eléctrica of 3.14e-07 Ω·m | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
300 °C | 4.02e-07 Ω·m Show Material materials with Resistividad eléctrica of 4.02e-07 Ω·m | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
400 °C | 5.02e-07 Ω·m Show Material materials with Resistividad eléctrica of 5.02e-07 Ω·m | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
500 °C | 6.21e-07 Ω·m Show Material materials with Resistividad eléctrica of 6.21e-07 Ω·m | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire | ||
600 °C | 7.55e-07 Ω·m Show Material materials with Resistividad eléctrica of 7.55e-07 Ω·m | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire |
Magnético
Property | Value | Comment |
---|---|---|
Temperatura de Curie | 770 °C Show Material materials with Temperatura de Curie of 770 °C | Typical for Low Carbon Steel |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Azufre | 0.035 % Show Material materials with Azufre of 0.035 % | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire |
Carbono | 0.21 % Show Material materials with Carbono of 0.21 % | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire |
Cobre | 0.55 % Show Material materials with Cobre of 0.55 % | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire |
Fósforo | 0.035 % Show Material materials with Fósforo of 0.035 % | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire |
Manganeso | 1.5 % Show Material materials with Manganeso of 1.5 % | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire |
Nitrógeno | 0.012 % Show Material materials with Nitrógeno of 0.012 % | normalized or normalized formed (+N) | EN 10025-2, EN 10025 | Strip, Sheet, Flat, Rod, Wire |