General
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Densidad | 20 °C | 7.848 - 7.85 g/cm³ Show Material materials with Densidad of 7.848 - 7.85 g/cm³ | quenched and tempered (+QT) | EN 10028-2 | Flat |
20 °C | 7.848 g/cm³ Show Material materials with Densidad of 7.848 g/cm³ | quenched and tempered (+QT) | EN 10028-2 | Flat | |
20 °C | 7.85 g/cm³ Show Material materials with Densidad of 7.85 g/cm³ | quenched and tempered (+QT) | EN 10028-2 | Flat | |
50 °C | 7.839 g/cm³ Show Material materials with Densidad of 7.839 g/cm³ | quenched and tempered (+QT) | EN 10028-2 | Flat | |
100 °C | 7.824 g/cm³ Show Material materials with Densidad of 7.824 g/cm³ | quenched and tempered (+QT) | EN 10028-2 | Flat | |
150 °C | 7.809 g/cm³ Show Material materials with Densidad of 7.809 g/cm³ | quenched and tempered (+QT) | EN 10028-2 | Flat | |
200 °C | 7.792 g/cm³ Show Material materials with Densidad of 7.792 g/cm³ | quenched and tempered (+QT) | EN 10028-2 | Flat | |
250 °C | 7.774 g/cm³ Show Material materials with Densidad of 7.774 g/cm³ | quenched and tempered (+QT) | EN 10028-2 | Flat | |
300 °C | 7.756 g/cm³ Show Material materials with Densidad of 7.756 g/cm³ | quenched and tempered (+QT) | EN 10028-2 | Flat | |
350 °C | 7.738 g/cm³ Show Material materials with Densidad of 7.738 g/cm³ | quenched and tempered (+QT) | EN 10028-2 | Flat | |
400 °C | 7.719 g/cm³ Show Material materials with Densidad of 7.719 g/cm³ | quenched and tempered (+QT) | EN 10028-2 | Flat | |
450 °C | 7.7 g/cm³ Show Material materials with Densidad of 7.7 g/cm³ | quenched and tempered (+QT) | EN 10028-2 | Flat | |
500 °C | 7.681 g/cm³ Show Material materials with Densidad of 7.681 g/cm³ | quenched and tempered (+QT) | EN 10028-2 | Flat | |
550 °C | 7.662 g/cm³ Show Material materials with Densidad of 7.662 g/cm³ | quenched and tempered (+QT) | EN 10028-2 | Flat | |
600 °C | 7.643 g/cm³ Show Material materials with Densidad of 7.643 g/cm³ | quenched and tempered (+QT) | EN 10028-2 | Flat |
Mecánica
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Coeficiente de Poisson | 20 °C | 0.283 [-] Show Material materials with Coeficiente de Poisson of 0.283 [-] | quenched and tempered (+QT) | EN 10028-2 | Flat | |
20 °C | 0.284 [-] Show Material materials with Coeficiente de Poisson of 0.284 [-] | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
50 °C | 0.284 [-] Show Material materials with Coeficiente de Poisson of 0.284 [-] | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
100 °C | 0.283 [-] Show Material materials with Coeficiente de Poisson of 0.283 [-] | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
150 °C | 0.285 [-] Show Material materials with Coeficiente de Poisson of 0.285 [-] | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
200 °C | 0.287 [-] Show Material materials with Coeficiente de Poisson of 0.287 [-] | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
250 °C | 0.29 [-] Show Material materials with Coeficiente de Poisson of 0.29 [-] | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
300 °C | 0.292 [-] Show Material materials with Coeficiente de Poisson of 0.292 [-] | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
350 °C | 0.295 [-] Show Material materials with Coeficiente de Poisson of 0.295 [-] | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
400 °C | 0.296 [-] Show Material materials with Coeficiente de Poisson of 0.296 [-] | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
450 °C | 0.299 [-] Show Material materials with Coeficiente de Poisson of 0.299 [-] | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
500 °C | 0.301 [-] Show Material materials with Coeficiente de Poisson of 0.301 [-] | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
550 °C | 0.305 [-] Show Material materials with Coeficiente de Poisson of 0.305 [-] | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
600 °C | 0.31 [-] Show Material materials with Coeficiente de Poisson of 0.31 [-] | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
Elongación | 16.6 % Show Material materials with Elongación of 16.6 % | Predicted Value, A80 Transverse | ||||
17.8 % Show Material materials with Elongación of 17.8 % | Predicted Value, A80 | |||||
18.0 % Show Material materials with Elongación of 18.0 % | Predicted Value, A200 | |||||
20.2 % Show Material materials with Elongación of 20.2 % | Predicted Value, A5 | |||||
24.8 % Show Material materials with Elongación of 24.8 % | Predicted Value, A50 | |||||
20 °C | 19 % Show Material materials with Elongación of 19 % | quenched and tempered (+QT) | EN 10028-2 | Flat | Transverse | |
20 °C | 19 % Show Material materials with Elongación of 19 % | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
Estricción | 43.2 % Show Material materials with Estricción of 43.2 % | Predicted Value | ||||
43.9 % Show Material materials with Estricción of 43.9 % | Predicted Value, Transverse | |||||
Límite elástico | 256.7 MPa Show Material materials with Límite elástico of 256.7 MPa | Predicted Value, RP1 | ||||
265.2 MPa Show Material materials with Límite elástico of 265.2 MPa | Predicted Value, RP1 Transverse | |||||
365.1 MPa Show Material materials with Límite elástico of 365.1 MPa | Predicted Value, RP02 Transverse | |||||
366.9 MPa Show Material materials with Límite elástico of 366.9 MPa | Predicted Value, RP05 | |||||
481.7 MPa Show Material materials with Límite elástico of 481.7 MPa | Predicted Value, RP002 | |||||
20 °C | 245 MPa Show Material materials with Límite elástico of 245 MPa | quenched and tempered (+QT) | EN 10028-2 | Flat | Transverse | |
20 °C | 245 MPa Show Material materials with Límite elástico of 245 MPa | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
20 °C | 270 MPa Show Material materials with Límite elástico of 270 MPa | quenched and tempered (+QT) | EN 10028-2 | Flat | Transverse | |
50 °C | 235 MPa Show Material materials with Límite elástico of 235 MPa | quenched and tempered (+QT) | EN 10028-2 | Flat | RP02 | |
100 °C | 223 MPa Show Material materials with Límite elástico of 223 MPa | quenched and tempered (+QT) | EN 10028-2 | Flat | RP02 | |
150 °C | 215 MPa Show Material materials with Límite elástico of 215 MPa | quenched and tempered (+QT) | EN 10028-2 | Flat | RP02 | |
200 °C | 211 MPa Show Material materials with Límite elástico of 211 MPa | quenched and tempered (+QT) | EN 10028-2 | Flat | RP02 | |
250 °C | 199 MPa Show Material materials with Límite elástico of 199 MPa | quenched and tempered (+QT) | EN 10028-2 | Flat | RP02 | |
300 °C | 184 MPa Show Material materials with Límite elástico of 184 MPa | quenched and tempered (+QT) | EN 10028-2 | Flat | RP02 | |
350 °C | 170 MPa Show Material materials with Límite elástico of 170 MPa | quenched and tempered (+QT) | EN 10028-2 | Flat | RP02 | |
400 °C | 159 MPa Show Material materials with Límite elástico of 159 MPa | quenched and tempered (+QT) | EN 10028-2 | Flat | RP02 | |
450 °C | 148 MPa Show Material materials with Límite elástico of 148 MPa | quenched and tempered (+QT) | EN 10028-2 | Flat | RP02 | |
500 °C | 139 MPa Show Material materials with Límite elástico of 139 MPa | quenched and tempered (+QT) | EN 10028-2 | Flat | RP02 | |
Módulo de cizallamiento | 20 °C | 82.8 GPa Show Material materials with Módulo de cizallamiento of 82.8 GPa | quenched and tempered (+QT) | EN 10028-2 | Flat | |
50 °C | 82.4 GPa Show Material materials with Módulo de cizallamiento of 82.4 GPa | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
100 °C | 81.4 GPa Show Material materials with Módulo de cizallamiento of 81.4 GPa | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
150 °C | 80.0 GPa Show Material materials with Módulo de cizallamiento of 80.0 GPa | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
200 °C | 78.4 GPa Show Material materials with Módulo de cizallamiento of 78.4 GPa | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
250 °C | 76.6 GPa Show Material materials with Módulo de cizallamiento of 76.6 GPa | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
300 °C | 74.8 GPa Show Material materials with Módulo de cizallamiento of 74.8 GPa | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
350 °C | 73.1 GPa Show Material materials with Módulo de cizallamiento of 73.1 GPa | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
400 °C | 71.3 GPa Show Material materials with Módulo de cizallamiento of 71.3 GPa | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
450 °C | 69.5 GPa Show Material materials with Módulo de cizallamiento of 69.5 GPa | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
500 °C | 67.6 GPa Show Material materials with Módulo de cizallamiento of 67.6 GPa | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
550 °C | 65.6 GPa Show Material materials with Módulo de cizallamiento of 65.6 GPa | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
600 °C | 63.6 GPa Show Material materials with Módulo de cizallamiento of 63.6 GPa | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
Módulo elástico | -100 °C | 217 GPa Show Material materials with Módulo elástico of 217 GPa | quenched and tempered (+QT) | EN 10028-2 | Flat | |
20 °C | 212 GPa Show Material materials with Módulo elástico of 212 GPa | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
20 °C | 212 - 212.5 GPa Show Material materials with Módulo elástico of 212 - 212.5 GPa | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
20 °C | 212.5 GPa Show Material materials with Módulo elástico of 212.5 GPa | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
50 °C | 211.6 GPa Show Material materials with Módulo elástico of 211.6 GPa | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
100 °C | 207 - 209 GPa Show Material materials with Módulo elástico of 207 - 209 GPa | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
100 °C | 207 GPa Show Material materials with Módulo elástico of 207 GPa | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
100 °C | 207 - 208.9 GPa Show Material materials with Módulo elástico of 207 - 208.9 GPa | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
100 °C | 208.9 - 209 GPa Show Material materials with Módulo elástico of 208.9 - 209 GPa | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
100 °C | 208.9 GPa Show Material materials with Módulo elástico of 208.9 GPa | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
100 °C | 209 GPa Show Material materials with Módulo elástico of 209 GPa | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
150 °C | 205.5 GPa Show Material materials with Módulo elástico of 205.5 GPa | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
200 °C | 199 - 202 GPa Show Material materials with Módulo elástico of 199 - 202 GPa | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
200 °C | 199 GPa Show Material materials with Módulo elástico of 199 GPa | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
200 °C | 199 - 201.8 GPa Show Material materials with Módulo elástico of 199 - 201.8 GPa | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
200 °C | 201.8 - 202 GPa Show Material materials with Módulo elástico of 201.8 - 202 GPa | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
200 °C | 201.8 GPa Show Material materials with Módulo elástico of 201.8 GPa | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
200 °C | 202 GPa Show Material materials with Módulo elástico of 202 GPa | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
250 °C | 197.7 GPa Show Material materials with Módulo elástico of 197.7 GPa | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
300 °C | 192 - 193 GPa Show Material materials with Módulo elástico of 192 - 193 GPa | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
300 °C | 192 GPa Show Material materials with Módulo elástico of 192 GPa | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
300 °C | 192 - 193.4 GPa Show Material materials with Módulo elástico of 192 - 193.4 GPa | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
300 °C | 193 GPa Show Material materials with Módulo elástico of 193 GPa | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
300 °C | 193 - 193.4 GPa Show Material materials with Módulo elástico of 193 - 193.4 GPa | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
300 °C | 193.4 GPa Show Material materials with Módulo elástico of 193.4 GPa | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
350 °C | 189.2 GPa Show Material materials with Módulo elástico of 189.2 GPa | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
400 °C | 184 - 185 GPa Show Material materials with Módulo elástico of 184 - 185 GPa | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
400 °C | 184 GPa Show Material materials with Módulo elástico of 184 GPa | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
400 °C | 184 - 184.8 GPa Show Material materials with Módulo elástico of 184 - 184.8 GPa | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
400 °C | 184.8 - 185 GPa Show Material materials with Módulo elástico of 184.8 - 185 GPa | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
400 °C | 184.8 GPa Show Material materials with Módulo elástico of 184.8 GPa | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
400 °C | 185 GPa Show Material materials with Módulo elástico of 185 GPa | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
450 °C | 180.4 GPa Show Material materials with Módulo elástico of 180.4 GPa | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
500 °C | 175 - 176 GPa Show Material materials with Módulo elástico of 175 - 176 GPa | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
500 °C | 175 GPa Show Material materials with Módulo elástico of 175 GPa | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
500 °C | 175 - 175.9 GPa Show Material materials with Módulo elástico of 175 - 175.9 GPa | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
500 °C | 175.9 - 176 GPa Show Material materials with Módulo elástico of 175.9 - 176 GPa | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
500 °C | 175.9 GPa Show Material materials with Módulo elástico of 175.9 GPa | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
500 °C | 176 GPa Show Material materials with Módulo elástico of 176 GPa | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
550 °C | 171.3 GPa Show Material materials with Módulo elástico of 171.3 GPa | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
600 °C | 164 - 166 GPa Show Material materials with Módulo elástico of 164 - 166 GPa | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
600 °C | 164 GPa Show Material materials with Módulo elástico of 164 GPa | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
600 °C | 164 - 166.6 GPa Show Material materials with Módulo elástico of 164 - 166.6 GPa | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
600 °C | 166 GPa Show Material materials with Módulo elástico of 166 GPa | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
600 °C | 166 - 166.6 GPa Show Material materials with Módulo elástico of 166 - 166.6 GPa | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
600 °C | 166.6 GPa Show Material materials with Módulo elástico of 166.6 GPa | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
Resistencia a la tracción | 20 °C | 420 - 590 MPa Show Material materials with Resistencia a la tracción of 420 - 590 MPa | quenched and tempered (+QT) | EN 10028-2 | Flat | Transverse |
20 °C | 420 - 570 MPa Show Material materials with Resistencia a la tracción of 420 - 570 MPa | quenched and tempered (+QT) | EN 10028-2 | Flat | Transverse | |
20 °C | 420 - 570 MPa Show Material materials with Resistencia a la tracción of 420 - 570 MPa | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
20 °C | 440 - 590 MPa Show Material materials with Resistencia a la tracción of 440 - 590 MPa | quenched and tempered (+QT) | EN 10028-2 | Flat | Transverse | |
20 °C | 440 - 570 MPa Show Material materials with Resistencia a la tracción of 440 - 570 MPa | quenched and tempered (+QT) | EN 10028-2 | Flat | Transverse | |
Resistencia al cizallamiento | 602.2 MPa Show Material materials with Resistencia al cizallamiento of 602.2 MPa | Predicted Value |
Aplicaciones térmicas
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Calor específico | -100 °C | 423 J/(kg·K) Show Material materials with Calor específico of 423 J/(kg·K) | quenched and tempered (+QT) | EN 10028-2 | Flat | |
20 °C | 430 J/(kg·K) Show Material materials with Calor específico of 430 J/(kg·K) | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
20 °C | 430 - 461 J/(kg·K) Show Material materials with Calor específico of 430 - 461 J/(kg·K) | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
20 °C | 461 J/(kg·K) Show Material materials with Calor específico of 461 J/(kg·K) | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
100 °C | 479 - 500 J/(kg·K) Show Material materials with Calor específico of 479 - 500 J/(kg·K) | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
100 °C | 479 J/(kg·K) Show Material materials with Calor específico of 479 J/(kg·K) | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
100 °C | 500 J/(kg·K) Show Material materials with Calor específico of 500 J/(kg·K) | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
200 °C | 499 - 540 J/(kg·K) Show Material materials with Calor específico of 499 - 540 J/(kg·K) | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
200 °C | 499 J/(kg·K) Show Material materials with Calor específico of 499 J/(kg·K) | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
200 °C | 540 J/(kg·K) Show Material materials with Calor específico of 540 J/(kg·K) | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
300 °C | 517 - 580 J/(kg·K) Show Material materials with Calor específico of 517 - 580 J/(kg·K) | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
300 °C | 517 J/(kg·K) Show Material materials with Calor específico of 517 J/(kg·K) | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
300 °C | 580 J/(kg·K) Show Material materials with Calor específico of 580 J/(kg·K) | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
400 °C | 536 - 620 J/(kg·K) Show Material materials with Calor específico of 536 - 620 J/(kg·K) | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
400 °C | 536 J/(kg·K) Show Material materials with Calor específico of 536 J/(kg·K) | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
400 °C | 620 J/(kg·K) Show Material materials with Calor específico of 620 J/(kg·K) | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
500 °C | 558 - 690 J/(kg·K) Show Material materials with Calor específico of 558 - 690 J/(kg·K) | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
500 °C | 558 J/(kg·K) Show Material materials with Calor específico of 558 J/(kg·K) | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
500 °C | 690 J/(kg·K) Show Material materials with Calor específico of 690 J/(kg·K) | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
600 °C | 587 - 780 J/(kg·K) Show Material materials with Calor específico of 587 - 780 J/(kg·K) | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
600 °C | 587 J/(kg·K) Show Material materials with Calor específico of 587 J/(kg·K) | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
600 °C | 780 J/(kg·K) Show Material materials with Calor específico of 780 J/(kg·K) | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
Coeficiente de dilatación térmica | -100 °C | 1.05e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 1.05e-05 1/K | quenched and tempered (+QT) | EN 10028-2 | Flat | |
20 °C | 1.15e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 1.15e-05 1/K | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
100 °C | 1.21e-05 - 1.22e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 1.21e-05 - 1.22e-05 1/K | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
100 °C | 1.21e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 1.21e-05 1/K | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
100 °C | 1.22e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 1.22e-05 1/K | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
200 °C | 1.27e-05 - 1.29e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 1.27e-05 - 1.29e-05 1/K | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
200 °C | 1.27e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 1.27e-05 1/K | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
200 °C | 1.29e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 1.29e-05 1/K | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
300 °C | 1.32e-05 - 1.34e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 1.32e-05 - 1.34e-05 1/K | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
300 °C | 1.32e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 1.32e-05 1/K | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
300 °C | 1.34e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 1.34e-05 1/K | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
400 °C | 1.36e-05 - 1.4e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 1.36e-05 - 1.4e-05 1/K | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
400 °C | 1.36e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 1.36e-05 1/K | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
400 °C | 1.4e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 1.4e-05 1/K | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
500 °C | 1.4e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 1.4e-05 1/K | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
500 °C | 1.4e-05 - 1.43e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 1.4e-05 - 1.43e-05 1/K | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
500 °C | 1.43e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 1.43e-05 1/K | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
600 °C | 1.44e-05 - 1.46e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 1.44e-05 - 1.46e-05 1/K | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
600 °C | 1.44e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 1.44e-05 1/K | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
600 °C | 1.46e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 1.46e-05 1/K | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
Conductividad térmica | 20 °C | 45.9 - 46 W/(m·K) Show Material materials with Conductividad térmica of 45.9 - 46 W/(m·K) | quenched and tempered (+QT) | EN 10028-2 | Flat | |
20 °C | 45.9 W/(m·K) Show Material materials with Conductividad térmica of 45.9 W/(m·K) | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
20 °C | 46 W/(m·K) Show Material materials with Conductividad térmica of 46 W/(m·K) | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
100 °C | 46 W/(m·K) Show Material materials with Conductividad térmica of 46 W/(m·K) | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
100 °C | 46 - 46.4 W/(m·K) Show Material materials with Conductividad térmica of 46 - 46.4 W/(m·K) | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
100 °C | 46.4 W/(m·K) Show Material materials with Conductividad térmica of 46.4 W/(m·K) | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
200 °C | 45.6 - 46 W/(m·K) Show Material materials with Conductividad térmica of 45.6 - 46 W/(m·K) | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
200 °C | 45.6 W/(m·K) Show Material materials with Conductividad térmica of 45.6 W/(m·K) | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
200 °C | 46 W/(m·K) Show Material materials with Conductividad térmica of 46 W/(m·K) | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
300 °C | 43 W/(m·K) Show Material materials with Conductividad térmica of 43 W/(m·K) | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
300 °C | 43 - 43.5 W/(m·K) Show Material materials with Conductividad térmica of 43 - 43.5 W/(m·K) | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
300 °C | 43.5 W/(m·K) Show Material materials with Conductividad térmica of 43.5 W/(m·K) | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
400 °C | 40.9 - 41 W/(m·K) Show Material materials with Conductividad térmica of 40.9 - 41 W/(m·K) | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
400 °C | 40.9 W/(m·K) Show Material materials with Conductividad térmica of 40.9 W/(m·K) | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
400 °C | 41 W/(m·K) Show Material materials with Conductividad térmica of 41 W/(m·K) | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
500 °C | 38 W/(m·K) Show Material materials with Conductividad térmica of 38 W/(m·K) | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
500 °C | 38 - 38.2 W/(m·K) Show Material materials with Conductividad térmica of 38 - 38.2 W/(m·K) | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
500 °C | 38.2 W/(m·K) Show Material materials with Conductividad térmica of 38.2 W/(m·K) | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
600 °C | 35.5 - 36 W/(m·K) Show Material materials with Conductividad térmica of 35.5 - 36 W/(m·K) | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
600 °C | 35.5 W/(m·K) Show Material materials with Conductividad térmica of 35.5 W/(m·K) | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
600 °C | 36 W/(m·K) Show Material materials with Conductividad térmica of 36 W/(m·K) | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
Difusividad térmica | 20 °C | 12.7 mm²/s Show Material materials with Difusividad térmica of 12.7 mm²/s | quenched and tempered (+QT) | EN 10028-2 | Flat | |
100 °C | 12 mm²/s Show Material materials with Difusividad térmica of 12 mm²/s | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
200 °C | 11 mm²/s Show Material materials with Difusividad térmica of 11 mm²/s | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
300 °C | 9.9 mm²/s Show Material materials with Difusividad térmica of 9.9 mm²/s | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
400 °C | 8.7 mm²/s Show Material materials with Difusividad térmica of 8.7 mm²/s | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
500 °C | 7.3 mm²/s Show Material materials with Difusividad térmica of 7.3 mm²/s | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
600 °C | 6 mm²/s Show Material materials with Difusividad térmica of 6 mm²/s | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
Temperatura de fusión | 1382 - 1529 °C Show Material materials with Temperatura de fusión of 1382 - 1529 °C | Typical for Chromium Molybdenum Steel |
Eléctrico
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Conductividad eléctrica | 4 S/m Show Material materials with Conductividad eléctrica of 4 S/m | Predicted Value | ||||
Resistividad eléctrica | 20 °C | 2.27e-07 - 2.3e-07 Ω·m Show Material materials with Resistividad eléctrica of 2.27e-07 - 2.3e-07 Ω·m | quenched and tempered (+QT) | EN 10028-2 | Flat | |
20 °C | 2.27e-07 Ω·m Show Material materials with Resistividad eléctrica of 2.27e-07 Ω·m | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
20 °C | 2.27e-07 - 2.37e-07 Ω·m Show Material materials with Resistividad eléctrica of 2.27e-07 - 2.37e-07 Ω·m | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
20 °C | 2.3e-07 Ω·m Show Material materials with Resistividad eléctrica of 2.3e-07 Ω·m | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
20 °C | 2.3e-07 - 2.37e-07 Ω·m Show Material materials with Resistividad eléctrica of 2.3e-07 - 2.37e-07 Ω·m | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
20 °C | 2.37e-07 Ω·m Show Material materials with Resistividad eléctrica of 2.37e-07 Ω·m | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
50 °C | 2.56e-07 Ω·m Show Material materials with Resistividad eléctrica of 2.56e-07 Ω·m | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
100 °C | 2.76e-07 - 2.8e-07 Ω·m Show Material materials with Resistividad eléctrica of 2.76e-07 - 2.8e-07 Ω·m | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
100 °C | 2.76e-07 Ω·m Show Material materials with Resistividad eléctrica of 2.76e-07 Ω·m | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
100 °C | 2.76e-07 - 2.88e-07 Ω·m Show Material materials with Resistividad eléctrica of 2.76e-07 - 2.88e-07 Ω·m | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
100 °C | 2.8e-07 Ω·m Show Material materials with Resistividad eléctrica of 2.8e-07 Ω·m | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
100 °C | 2.8e-07 - 2.88e-07 Ω·m Show Material materials with Resistividad eléctrica of 2.8e-07 - 2.88e-07 Ω·m | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
100 °C | 2.88e-07 Ω·m Show Material materials with Resistividad eléctrica of 2.88e-07 Ω·m | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
150 °C | 3.21e-07 Ω·m Show Material materials with Resistividad eléctrica of 3.21e-07 Ω·m | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
200 °C | 3.46e-07 - 3.5e-07 Ω·m Show Material materials with Resistividad eléctrica of 3.46e-07 - 3.5e-07 Ω·m | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
200 °C | 3.46e-07 Ω·m Show Material materials with Resistividad eléctrica of 3.46e-07 Ω·m | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
200 °C | 3.46e-07 - 3.59e-07 Ω·m Show Material materials with Resistividad eléctrica of 3.46e-07 - 3.59e-07 Ω·m | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
200 °C | 3.5e-07 Ω·m Show Material materials with Resistividad eléctrica of 3.5e-07 Ω·m | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
200 °C | 3.5e-07 - 3.59e-07 Ω·m Show Material materials with Resistividad eléctrica of 3.5e-07 - 3.59e-07 Ω·m | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
200 °C | 3.59e-07 Ω·m Show Material materials with Resistividad eléctrica of 3.59e-07 Ω·m | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
250 °C | 4.01e-07 Ω·m Show Material materials with Resistividad eléctrica of 4.01e-07 Ω·m | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
300 °C | 4.3e-07 Ω·m Show Material materials with Resistividad eléctrica of 4.3e-07 Ω·m | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
300 °C | 4.3e-07 - 4.31e-07 Ω·m Show Material materials with Resistividad eléctrica of 4.3e-07 - 4.31e-07 Ω·m | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
300 °C | 4.3e-07 - 4.45e-07 Ω·m Show Material materials with Resistividad eléctrica of 4.3e-07 - 4.45e-07 Ω·m | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
300 °C | 4.31e-07 Ω·m Show Material materials with Resistividad eléctrica of 4.31e-07 Ω·m | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
300 °C | 4.31e-07 - 4.45e-07 Ω·m Show Material materials with Resistividad eléctrica of 4.31e-07 - 4.45e-07 Ω·m | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
300 °C | 4.45e-07 Ω·m Show Material materials with Resistividad eléctrica of 4.45e-07 Ω·m | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
350 °C | 4.95e-07 Ω·m Show Material materials with Resistividad eléctrica of 4.95e-07 Ω·m | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
400 °C | 5.3e-07 Ω·m Show Material materials with Resistividad eléctrica of 5.3e-07 Ω·m | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
400 °C | 5.3e-07 - 5.32e-07 Ω·m Show Material materials with Resistividad eléctrica of 5.3e-07 - 5.32e-07 Ω·m | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
400 °C | 5.3e-07 - 5.48e-07 Ω·m Show Material materials with Resistividad eléctrica of 5.3e-07 - 5.48e-07 Ω·m | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
400 °C | 5.32e-07 Ω·m Show Material materials with Resistividad eléctrica of 5.32e-07 Ω·m | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
400 °C | 5.32e-07 - 5.48e-07 Ω·m Show Material materials with Resistividad eléctrica of 5.32e-07 - 5.48e-07 Ω·m | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
400 °C | 5.48e-07 Ω·m Show Material materials with Resistividad eléctrica of 5.48e-07 Ω·m | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
450 °C | 6.06e-07 Ω·m Show Material materials with Resistividad eléctrica of 6.06e-07 Ω·m | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
500 °C | 6.48e-07 - 6.5e-07 Ω·m Show Material materials with Resistividad eléctrica of 6.48e-07 - 6.5e-07 Ω·m | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
500 °C | 6.48e-07 Ω·m Show Material materials with Resistividad eléctrica of 6.48e-07 Ω·m | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
500 °C | 6.48e-07 - 6.63e-07 Ω·m Show Material materials with Resistividad eléctrica of 6.48e-07 - 6.63e-07 Ω·m | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
500 °C | 6.5e-07 Ω·m Show Material materials with Resistividad eléctrica of 6.5e-07 Ω·m | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
500 °C | 6.5e-07 - 6.63e-07 Ω·m Show Material materials with Resistividad eléctrica of 6.5e-07 - 6.63e-07 Ω·m | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
500 °C | 6.63e-07 Ω·m Show Material materials with Resistividad eléctrica of 6.63e-07 Ω·m | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
550 °C | 7.28e-07 Ω·m Show Material materials with Resistividad eléctrica of 7.28e-07 Ω·m | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
600 °C | 7.8e-07 Ω·m Show Material materials with Resistividad eléctrica of 7.8e-07 Ω·m | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
600 °C | 7.8e-07 - 7.81e-07 Ω·m Show Material materials with Resistividad eléctrica of 7.8e-07 - 7.81e-07 Ω·m | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
600 °C | 7.8e-07 - 7.97e-07 Ω·m Show Material materials with Resistividad eléctrica of 7.8e-07 - 7.97e-07 Ω·m | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
600 °C | 7.81e-07 Ω·m Show Material materials with Resistividad eléctrica of 7.81e-07 Ω·m | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
600 °C | 7.81e-07 - 7.97e-07 Ω·m Show Material materials with Resistividad eléctrica of 7.81e-07 - 7.97e-07 Ω·m | quenched and tempered (+QT) | EN 10028-2 | Flat | ||
600 °C | 7.97e-07 Ω·m Show Material materials with Resistividad eléctrica of 7.97e-07 Ω·m | quenched and tempered (+QT) | EN 10028-2 | Flat |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Azufre | 0.01 % Show Material materials with Azufre of 0.01 % | quenched and tempered (+QT) | EN 10028-2 | Flat |
Carbono | 0.08 - 0.18 % Show Material materials with Carbono of 0.08 - 0.18 % | quenched and tempered (+QT) | EN 10028-2 | Flat |
Cobre | 0.3 % Show Material materials with Cobre of 0.3 % | quenched and tempered (+QT) | EN 10028-2 | Flat |
Cromo | 0.7 - 1.15 % Show Material materials with Cromo of 0.7 - 1.15 % | quenched and tempered (+QT) | EN 10028-2 | Flat |
Fósforo | 0.025 % Show Material materials with Fósforo of 0.025 % | quenched and tempered (+QT) | EN 10028-2 | Flat |
Manganeso | 0.4 - 1 % Show Material materials with Manganeso of 0.4 - 1 % | quenched and tempered (+QT) | EN 10028-2 | Flat |
Molibdeno | 0.4 - 0.6 % Show Material materials with Molibdeno of 0.4 - 0.6 % | quenched and tempered (+QT) | EN 10028-2 | Flat |
Nitrógeno | 0.012 % Show Material materials with Nitrógeno of 0.012 % | quenched and tempered (+QT) | EN 10028-2 | Flat |
Silicona | 0.35 % Show Material materials with Silicona of 0.35 % | quenched and tempered (+QT) | EN 10028-2 | Flat |
Technological properties
Property | ||
---|---|---|
Supplier Disclaimer | The given information is a rough description and some properties can depend on various factors such as product thickness. Please contact the supplier or refer to the related norm or standard for further information. |