General
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Densidad | 20 °C | 7.85 g/cm³ Show Material materials with Densidad of 7.85 g/cm³ | skin passed | EN 10130 | Sheet, Flat, Bar, Strip |
Mecánica
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Coeficiente de Poisson | 20 °C | 0.284 [-] Show Material materials with Coeficiente de Poisson of 0.284 [-] | skin passed | EN 10130 | Sheet, Flat, Bar, Strip | |
Dureza Brinell | 272 [-] Show Material materials with Dureza Brinell of 272 [-] | Predicted Value, Transverse | ||||
Elongación | 18.6 % Show Material materials with Elongación of 18.6 % | Predicted Value, Transverse | ||||
20.2 % Show Material materials with Elongación of 20.2 % | Predicted Value, A200 | |||||
22.3 % Show Material materials with Elongación of 22.3 % | Predicted Value, A5 | |||||
22.5 % Show Material materials with Elongación of 22.5 % | Predicted Value, A80 Transverse | |||||
37.2 % Show Material materials with Elongación of 37.2 % | Predicted Value | |||||
39.4 % Show Material materials with Elongación of 39.4 % | Predicted Value, A50 | |||||
20 °C | 38 % Show Material materials with Elongación of 38 % | skin passed | EN 10130 | Sheet, Flat, Bar, Strip | A80 | |
20 °C | 41 % Show Material materials with Elongación of 41 % | skin passed | EN 10130 | Sheet, Flat, Bar, Strip | A80 | |
Estricción | 42.9 % Show Material materials with Estricción of 42.9 % | Predicted Value, Transverse | ||||
47.3 % Show Material materials with Estricción of 47.3 % | Predicted Value | |||||
Límite elástico | 280.5 MPa Show Material materials with Límite elástico of 280.5 MPa | Predicted Value, RP1 | ||||
280.5 MPa Show Material materials with Límite elástico of 280.5 MPa | Predicted Value, Transverse | |||||
317.2 MPa Show Material materials with Límite elástico of 317.2 MPa | Predicted Value, RP1 Transverse | |||||
318.5 MPa Show Material materials with Límite elástico of 318.5 MPa | Predicted Value, RP05 | |||||
323.2 MPa Show Material materials with Límite elástico of 323.2 MPa | Predicted Value, RP02 | |||||
478.6 MPa Show Material materials with Límite elástico of 478.6 MPa | Predicted Value, RP02 Transverse | |||||
494.9 MPa Show Material materials with Límite elástico of 494.9 MPa | Predicted Value, RP002 | |||||
20 °C | 120 - 180 MPa Show Material materials with Límite elástico of 120 - 180 MPa | skin passed | EN 10130 | Sheet, Flat, Bar, Strip | ||
20 °C | 120 - 170 MPa Show Material materials with Límite elástico of 120 - 170 MPa | skin passed | EN 10130 | Sheet, Flat, Bar, Strip | ||
Módulo de cizallamiento | 82 GPa Show Material materials with Módulo de cizallamiento of 82 GPa | Typical for Low Carbon Steel | ||||
Módulo elástico | -100 °C | 217 GPa Show Material materials with Módulo elástico of 217 GPa | skin passed | EN 10130 | Sheet, Flat, Bar, Strip | |
20 °C | 212 GPa Show Material materials with Módulo elástico of 212 GPa | skin passed | EN 10130 | Sheet, Flat, Bar, Strip | ||
100 °C | 207 GPa Show Material materials with Módulo elástico of 207 GPa | skin passed | EN 10130 | Sheet, Flat, Bar, Strip | ||
200 °C | 199 GPa Show Material materials with Módulo elástico of 199 GPa | skin passed | EN 10130 | Sheet, Flat, Bar, Strip | ||
300 °C | 192 GPa Show Material materials with Módulo elástico of 192 GPa | skin passed | EN 10130 | Sheet, Flat, Bar, Strip | ||
400 °C | 184 GPa Show Material materials with Módulo elástico of 184 GPa | skin passed | EN 10130 | Sheet, Flat, Bar, Strip | ||
500 °C | 175 GPa Show Material materials with Módulo elástico of 175 GPa | skin passed | EN 10130 | Sheet, Flat, Bar, Strip | ||
600 °C | 164 GPa Show Material materials with Módulo elástico of 164 GPa | skin passed | EN 10130 | Sheet, Flat, Bar, Strip | ||
Resistencia a la tracción | 20 °C | 270 - 350 MPa Show Material materials with Resistencia a la tracción of 270 - 350 MPa | skin passed | EN 10130 | Sheet, Flat, Bar, Strip | |
20 °C | 270 - 330 MPa Show Material materials with Resistencia a la tracción of 270 - 330 MPa | skin passed | EN 10130 | Sheet, Flat, Bar, Strip | ||
Resistencia al cizallamiento | 544.1 MPa Show Material materials with Resistencia al cizallamiento of 544.1 MPa | Predicted Value |
Aplicaciones térmicas
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Calor específico | -100 °C | 423 J/(kg·K) Show Material materials with Calor específico of 423 J/(kg·K) | skin passed | EN 10130 | Sheet, Flat, Bar, Strip | |
20 °C | 461 J/(kg·K) Show Material materials with Calor específico of 461 J/(kg·K) | skin passed | EN 10130 | Sheet, Flat, Bar, Strip | ||
100 °C | 479 J/(kg·K) Show Material materials with Calor específico of 479 J/(kg·K) | skin passed | EN 10130 | Sheet, Flat, Bar, Strip | ||
200 °C | 499 J/(kg·K) Show Material materials with Calor específico of 499 J/(kg·K) | skin passed | EN 10130 | Sheet, Flat, Bar, Strip | ||
300 °C | 517 J/(kg·K) Show Material materials with Calor específico of 517 J/(kg·K) | skin passed | EN 10130 | Sheet, Flat, Bar, Strip | ||
400 °C | 536 J/(kg·K) Show Material materials with Calor específico of 536 J/(kg·K) | skin passed | EN 10130 | Sheet, Flat, Bar, Strip | ||
500 °C | 558 J/(kg·K) Show Material materials with Calor específico of 558 J/(kg·K) | skin passed | EN 10130 | Sheet, Flat, Bar, Strip | ||
600 °C | 587 J/(kg·K) Show Material materials with Calor específico of 587 J/(kg·K) | skin passed | EN 10130 | Sheet, Flat, Bar, Strip | ||
Coeficiente de dilatación térmica | -100 °C | 1.08e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 1.08e-05 1/K | skin passed | EN 10130 | Sheet, Flat, Bar, Strip | |
20 °C | 1.19e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 1.19e-05 1/K | skin passed | EN 10130 | Sheet, Flat, Bar, Strip | ||
100 °C | 1.25e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 1.25e-05 1/K | skin passed | EN 10130 | Sheet, Flat, Bar, Strip | ||
200 °C | 1.3e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 1.3e-05 1/K | skin passed | EN 10130 | Sheet, Flat, Bar, Strip | ||
300 °C | 1.36e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 1.36e-05 1/K | skin passed | EN 10130 | Sheet, Flat, Bar, Strip | ||
400 °C | 1.41e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 1.41e-05 1/K | skin passed | EN 10130 | Sheet, Flat, Bar, Strip | ||
500 °C | 1.45e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 1.45e-05 1/K | skin passed | EN 10130 | Sheet, Flat, Bar, Strip | ||
600 °C | 1.49e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 1.49e-05 1/K | skin passed | EN 10130 | Sheet, Flat, Bar, Strip | ||
Conductividad térmica | 20 °C | 57.5 W/(m·K) Show Material materials with Conductividad térmica of 57.5 W/(m·K) | skin passed | EN 10130 | Sheet, Flat, Bar, Strip | |
100 °C | 55.7 W/(m·K) Show Material materials with Conductividad térmica of 55.7 W/(m·K) | skin passed | EN 10130 | Sheet, Flat, Bar, Strip | ||
200 °C | 51.9 W/(m·K) Show Material materials with Conductividad térmica of 51.9 W/(m·K) | skin passed | EN 10130 | Sheet, Flat, Bar, Strip | ||
300 °C | 47.6 W/(m·K) Show Material materials with Conductividad térmica of 47.6 W/(m·K) | skin passed | EN 10130 | Sheet, Flat, Bar, Strip | ||
400 °C | 43.4 W/(m·K) Show Material materials with Conductividad térmica of 43.4 W/(m·K) | skin passed | EN 10130 | Sheet, Flat, Bar, Strip | ||
500 °C | 39.6 W/(m·K) Show Material materials with Conductividad térmica of 39.6 W/(m·K) | skin passed | EN 10130 | Sheet, Flat, Bar, Strip | ||
600 °C | 36 W/(m·K) Show Material materials with Conductividad térmica of 36 W/(m·K) | skin passed | EN 10130 | Sheet, Flat, Bar, Strip | ||
Difusividad térmica | 20 °C | 15.9 mm²/s Show Material materials with Difusividad térmica of 15.9 mm²/s | skin passed | EN 10130 | Sheet, Flat, Bar, Strip | |
100 °C | 14.3 mm²/s Show Material materials with Difusividad térmica of 14.3 mm²/s | skin passed | EN 10130 | Sheet, Flat, Bar, Strip | ||
200 °C | 12.5 mm²/s Show Material materials with Difusividad térmica of 12.5 mm²/s | skin passed | EN 10130 | Sheet, Flat, Bar, Strip | ||
300 °C | 10.8 mm²/s Show Material materials with Difusividad térmica of 10.8 mm²/s | skin passed | EN 10130 | Sheet, Flat, Bar, Strip | ||
400 °C | 9.2 mm²/s Show Material materials with Difusividad térmica of 9.2 mm²/s | skin passed | EN 10130 | Sheet, Flat, Bar, Strip | ||
500 °C | 7.6 mm²/s Show Material materials with Difusividad térmica of 7.6 mm²/s | skin passed | EN 10130 | Sheet, Flat, Bar, Strip | ||
600 °C | 6.1 mm²/s Show Material materials with Difusividad térmica of 6.1 mm²/s | skin passed | EN 10130 | Sheet, Flat, Bar, Strip | ||
Temperatura de fusión | 1480 - 1526 °C Show Material materials with Temperatura de fusión of 1480 - 1526 °C | Typical for Low Carbon Steel | ||||
Temperatura máx. de funcionamiento | 383.1 °C Show Material materials with Temperatura máx. de funcionamiento of 383.1 °C | Predicted Value, Long | ||||
500 °C Show Material materials with Temperatura máx. de funcionamiento of 500 °C | Typical for Carbon Steel |
Eléctrico
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Conductividad eléctrica | 8 S/m Show Material materials with Conductividad eléctrica of 8 S/m | Predicted Value | ||||
Resistividad eléctrica | 20 °C | 1.1e-07 Ω·m Show Material materials with Resistividad eléctrica of 1.1e-07 Ω·m | skin passed | EN 10130 | Sheet, Flat, Bar, Strip | |
100 °C | 2.3e-07 Ω·m Show Material materials with Resistividad eléctrica of 2.3e-07 Ω·m | skin passed | EN 10130 | Sheet, Flat, Bar, Strip | ||
200 °C | 3.04e-07 Ω·m Show Material materials with Resistividad eléctrica of 3.04e-07 Ω·m | skin passed | EN 10130 | Sheet, Flat, Bar, Strip | ||
300 °C | 3.94e-07 Ω·m Show Material materials with Resistividad eléctrica of 3.94e-07 Ω·m | skin passed | EN 10130 | Sheet, Flat, Bar, Strip | ||
400 °C | 5.01e-07 Ω·m Show Material materials with Resistividad eléctrica of 5.01e-07 Ω·m | skin passed | EN 10130 | Sheet, Flat, Bar, Strip | ||
500 °C | 6.25e-07 Ω·m Show Material materials with Resistividad eléctrica of 6.25e-07 Ω·m | skin passed | EN 10130 | Sheet, Flat, Bar, Strip | ||
600 °C | 7.7e-07 Ω·m Show Material materials with Resistividad eléctrica of 7.7e-07 Ω·m | skin passed | EN 10130 | Sheet, Flat, Bar, Strip |
Magnético
Property | Value | Comment |
---|---|---|
Temperatura de Curie | 770 °C Show Material materials with Temperatura de Curie of 770 °C | Typical for Low Carbon Steel |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Azufre | 0.02 % Show Material materials with Azufre of 0.02 % | skin passed | EN 10130 | Sheet, Flat, Bar, Strip |
Carbono | 0.02 % Show Material materials with Carbono of 0.02 % | skin passed | EN 10130 | Sheet, Flat, Bar, Strip |
Fósforo | 0.02 % Show Material materials with Fósforo of 0.02 % | skin passed | EN 10130 | Sheet, Flat, Bar, Strip |
Manganeso | 0.25 % Show Material materials with Manganeso of 0.25 % | skin passed | EN 10130 | Sheet, Flat, Bar, Strip |
Titanio | 0.3 % Show Material materials with Titanio of 0.3 % | skin passed | EN 10130 | Sheet, Flat, Bar, Strip |