General
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Densidad | 20 °C | 7.85 g/cm³ Show Material materials with Densidad of 7.85 g/cm³ | normalized or normalized formed (+N) | EN 10025-5, EN 10155, EN 10025-1 | Strip, Sheet, Flat, Rod, Wire, Bar |
Mecánica
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Coeficiente de Poisson | 20 °C | 0.284 [-] Show Material materials with Coeficiente de Poisson of 0.284 [-] | normalized or normalized formed (+N) | EN 10025-5, EN 10155, EN 10025-1 | Strip, Sheet, Flat, Rod, Wire, Bar | |
Elongación | 18.4 % Show Material materials with Elongación of 18.4 % | Predicted Value, A200 | ||||
22.1 % Show Material materials with Elongación of 22.1 % | Predicted Value, A5 | |||||
24.4 % Show Material materials with Elongación of 24.4 % | Predicted Value, A50 | |||||
20 °C | 17 % Show Material materials with Elongación of 17 % | normalized or normalized formed (+N) | EN 10025-5, EN 10155, EN 10025-1 | Strip, Sheet, Flat, Rod, Wire, Bar | A80 Transverse | |
20 °C | 18 % Show Material materials with Elongación of 18 % | normalized or normalized formed (+N) | EN 10025-5, EN 10155, EN 10025-1 | Strip, Sheet, Flat, Rod, Wire, Bar | A80 Transverse | |
20 °C | 19 % Show Material materials with Elongación of 19 % | normalized or normalized formed (+N) | EN 10025-5, EN 10155, EN 10025-1 | Strip, Sheet, Flat, Rod, Wire, Bar | A80 Transverse | |
20 °C | 19 % Show Material materials with Elongación of 19 % | normalized or normalized formed (+N) | EN 10025-5, EN 10155, EN 10025-1 | Strip, Sheet, Flat, Rod, Wire, Bar | A80 | |
20 °C | 20 % Show Material materials with Elongación of 20 % | normalized or normalized formed (+N) | EN 10025-5, EN 10155, EN 10025-1 | Strip, Sheet, Flat, Rod, Wire, Bar | A80 | |
20 °C | 21 % Show Material materials with Elongación of 21 % | normalized or normalized formed (+N) | EN 10025-5, EN 10155, EN 10025-1 | Strip, Sheet, Flat, Rod, Wire, Bar | A80 | |
20 °C | 22 % Show Material materials with Elongación of 22 % | normalized or normalized formed (+N) | EN 10025-5, EN 10155, EN 10025-1 | Strip, Sheet, Flat, Rod, Wire, Bar | Transverse | |
20 °C | 22 % Show Material materials with Elongación of 22 % | normalized or normalized formed (+N) | EN 10025-5, EN 10155 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 23 % Show Material materials with Elongación of 23 % | normalized or normalized formed (+N) | EN 10025-5, EN 10155, EN 10025-1 | Strip, Sheet, Flat, Rod, Wire, Bar | Transverse | |
20 °C | 24 % Show Material materials with Elongación of 24 % | normalized or normalized formed (+N) | EN 10025-5, EN 10155, EN 10025-1 | Strip, Sheet, Flat, Rod, Wire, Bar | Transverse | |
20 °C | 24 % Show Material materials with Elongación of 24 % | normalized or normalized formed (+N) | EN 10025-5, EN 10155, EN 10025-1 | Strip, Sheet, Flat, Rod, Wire, Bar | ||
20 °C | 25 % Show Material materials with Elongación of 25 % | normalized or normalized formed (+N) | EN 10025-5, EN 10155, EN 10025-1 | Strip, Sheet, Flat, Rod, Wire, Bar | ||
20 °C | 26 % Show Material materials with Elongación of 26 % | normalized or normalized formed (+N) | EN 10025-5, EN 10155, EN 10025-1 | Strip, Sheet, Flat, Rod, Wire, Bar | ||
Límite elástico | 249.4 MPa Show Material materials with Límite elástico of 249.4 MPa | Predicted Value, RP1 | ||||
278.8 MPa Show Material materials with Límite elástico of 278.8 MPa | Predicted Value, RP1 Transverse | |||||
288.4 MPa Show Material materials with Límite elástico of 288.4 MPa | Predicted Value, RP05 | |||||
318.4 MPa Show Material materials with Límite elástico of 318.4 MPa | Predicted Value, RP02 | |||||
346.3 MPa Show Material materials with Límite elástico of 346.3 MPa | Predicted Value, RP02 Transverse | |||||
467 MPa Show Material materials with Límite elástico of 467 MPa | Predicted Value, RP002 | |||||
20 °C | 195 MPa Show Material materials with Límite elástico of 195 MPa | normalized or normalized formed (+N) | EN 10025-5, EN 10155 | Strip, Sheet, Flat, Rod, Wire | Transverse | |
20 °C | 195 MPa Show Material materials with Límite elástico of 195 MPa | normalized or normalized formed (+N) | EN 10025-5, EN 10155 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 215 MPa Show Material materials with Límite elástico of 215 MPa | normalized or normalized formed (+N) | EN 10025-5, EN 10155 | Strip, Sheet, Flat, Rod, Wire | Transverse | |
20 °C | 215 MPa Show Material materials with Límite elástico of 215 MPa | normalized or normalized formed (+N) | EN 10025-5, EN 10155, EN 10025-1 | Strip, Sheet, Flat, Rod, Wire, Bar | ||
20 °C | 225 MPa Show Material materials with Límite elástico of 225 MPa | normalized or normalized formed (+N) | EN 10025-5, EN 10155 | Strip, Sheet, Flat, Rod, Wire | Transverse | |
20 °C | 225 MPa Show Material materials with Límite elástico of 225 MPa | normalized or normalized formed (+N) | EN 10025-5, EN 10155, EN 10025-1 | Strip, Sheet, Flat, Rod, Wire, Bar | ||
20 °C | 235 MPa Show Material materials with Límite elástico of 235 MPa | normalized or normalized formed (+N) | EN 10025-5, EN 10155 | Strip, Sheet, Flat, Rod, Wire | Transverse | |
20 °C | 235 MPa Show Material materials with Límite elástico of 235 MPa | normalized or normalized formed (+N) | EN 10025-5, EN 10155, EN 10025-1 | Strip, Sheet, Flat, Rod, Wire, Bar | ||
Módulo elástico | -100 °C | 217 GPa Show Material materials with Módulo elástico of 217 GPa | normalized or normalized formed (+N) | EN 10025-5, EN 10155, EN 10025-1 | Strip, Sheet, Flat, Rod, Wire, Bar | |
20 °C | 212 GPa Show Material materials with Módulo elástico of 212 GPa | normalized or normalized formed (+N) | EN 10025-5, EN 10155, EN 10025-1 | Strip, Sheet, Flat, Rod, Wire, Bar | ||
100 °C | 207 GPa Show Material materials with Módulo elástico of 207 GPa | normalized or normalized formed (+N) | EN 10025-5, EN 10155, EN 10025-1 | Strip, Sheet, Flat, Rod, Wire, Bar | ||
200 °C | 199 GPa Show Material materials with Módulo elástico of 199 GPa | normalized or normalized formed (+N) | EN 10025-5, EN 10155, EN 10025-1 | Strip, Sheet, Flat, Rod, Wire, Bar | ||
300 °C | 192 GPa Show Material materials with Módulo elástico of 192 GPa | normalized or normalized formed (+N) | EN 10025-5, EN 10155, EN 10025-1 | Strip, Sheet, Flat, Rod, Wire, Bar | ||
400 °C | 184 GPa Show Material materials with Módulo elástico of 184 GPa | normalized or normalized formed (+N) | EN 10025-5, EN 10155, EN 10025-1 | Strip, Sheet, Flat, Rod, Wire, Bar | ||
500 °C | 175 GPa Show Material materials with Módulo elástico of 175 GPa | normalized or normalized formed (+N) | EN 10025-5, EN 10155, EN 10025-1 | Strip, Sheet, Flat, Rod, Wire, Bar | ||
600 °C | 164 GPa Show Material materials with Módulo elástico of 164 GPa | normalized or normalized formed (+N) | EN 10025-5, EN 10155, EN 10025-1 | Strip, Sheet, Flat, Rod, Wire, Bar | ||
Resistencia a la tracción | 20 °C | 340 - 510 MPa Show Material materials with Resistencia a la tracción of 340 - 510 MPa | normalized or normalized formed (+N) | EN 10155, EN 10025-1, EN 10025-5 | Bar, Sheet, Strip, Flat | |
20 °C | 340 - 470 MPa Show Material materials with Resistencia a la tracción of 340 - 470 MPa | normalized or normalized formed (+N) | EN 10155, EN 10025-1, EN 10025-5 | Bar, Sheet, Strip, Flat | ||
20 °C | 350 - 510 MPa Show Material materials with Resistencia a la tracción of 350 - 510 MPa | normalized or normalized formed (+N) | EN 10025-5, EN 10155 | Strip, Sheet, Flat, Rod, Wire | Transverse | |
20 °C | 350 - 500 MPa Show Material materials with Resistencia a la tracción of 350 - 500 MPa | normalized or normalized formed (+N) | EN 10025-5, EN 10155 | Strip, Sheet, Flat, Rod, Wire | Transverse | |
20 °C | 350 - 510 MPa Show Material materials with Resistencia a la tracción of 350 - 510 MPa | normalized or normalized formed (+N) | EN 10025-5, EN 10155 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 350 - 500 MPa Show Material materials with Resistencia a la tracción of 350 - 500 MPa | normalized or normalized formed (+N) | EN 10025-5, EN 10155 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 360 - 510 MPa Show Material materials with Resistencia a la tracción of 360 - 510 MPa | normalized or normalized formed (+N) | EN 10025-5, EN 10155 | Strip, Sheet, Flat, Rod, Wire | Transverse | |
20 °C | 360 - 500 MPa Show Material materials with Resistencia a la tracción of 360 - 500 MPa | normalized or normalized formed (+N) | EN 10025-5, EN 10155 | Strip, Sheet, Flat, Rod, Wire | Transverse | |
20 °C | 360 - 510 MPa Show Material materials with Resistencia a la tracción of 360 - 510 MPa | normalized or normalized formed (+N) | EN 10025-5, EN 10155, EN 10025-1 | Strip, Sheet, Flat, Rod, Wire, Bar | ||
20 °C | 360 - 500 MPa Show Material materials with Resistencia a la tracción of 360 - 500 MPa | normalized or normalized formed (+N) | EN 10025-5, EN 10155 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 360 - 470 MPa Show Material materials with Resistencia a la tracción of 360 - 470 MPa | normalized or normalized formed (+N) | EN 10155, EN 10025-1, EN 10025-5 | Bar, Sheet, Strip, Flat |
Aplicaciones térmicas
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Calor específico | -100 °C | 423 J/(kg·K) Show Material materials with Calor específico of 423 J/(kg·K) | normalized or normalized formed (+N) | EN 10025-5, EN 10155, EN 10025-1 | Strip, Sheet, Flat, Rod, Wire, Bar |
20 °C | 461 J/(kg·K) Show Material materials with Calor específico of 461 J/(kg·K) | normalized or normalized formed (+N) | EN 10025-5, EN 10155, EN 10025-1 | Strip, Sheet, Flat, Rod, Wire, Bar | |
100 °C | 479 J/(kg·K) Show Material materials with Calor específico of 479 J/(kg·K) | normalized or normalized formed (+N) | EN 10025-5, EN 10155, EN 10025-1 | Strip, Sheet, Flat, Rod, Wire, Bar | |
200 °C | 499 J/(kg·K) Show Material materials with Calor específico of 499 J/(kg·K) | normalized or normalized formed (+N) | EN 10025-5, EN 10155, EN 10025-1 | Strip, Sheet, Flat, Rod, Wire, Bar | |
300 °C | 517 J/(kg·K) Show Material materials with Calor específico of 517 J/(kg·K) | normalized or normalized formed (+N) | EN 10025-5, EN 10155, EN 10025-1 | Strip, Sheet, Flat, Rod, Wire, Bar | |
400 °C | 536 J/(kg·K) Show Material materials with Calor específico of 536 J/(kg·K) | normalized or normalized formed (+N) | EN 10025-5, EN 10155, EN 10025-1 | Strip, Sheet, Flat, Rod, Wire, Bar | |
500 °C | 558 J/(kg·K) Show Material materials with Calor específico of 558 J/(kg·K) | normalized or normalized formed (+N) | EN 10025-5, EN 10155, EN 10025-1 | Strip, Sheet, Flat, Rod, Wire, Bar | |
600 °C | 587 J/(kg·K) Show Material materials with Calor específico of 587 J/(kg·K) | normalized or normalized formed (+N) | EN 10025-5, EN 10155, EN 10025-1 | Strip, Sheet, Flat, Rod, Wire, Bar | |
Coeficiente de dilatación térmica | -100 °C | 1.08e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 1.08e-05 1/K | normalized or normalized formed (+N) | EN 10025-5, EN 10155, EN 10025-1 | Strip, Sheet, Flat, Rod, Wire, Bar |
20 °C | 1.19e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 1.19e-05 1/K | normalized or normalized formed (+N) | EN 10025-5, EN 10155, EN 10025-1 | Strip, Sheet, Flat, Rod, Wire, Bar | |
100 °C | 1.25e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 1.25e-05 1/K | normalized or normalized formed (+N) | EN 10025-5, EN 10155, EN 10025-1 | Strip, Sheet, Flat, Rod, Wire, Bar | |
200 °C | 1.3e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 1.3e-05 1/K | normalized or normalized formed (+N) | EN 10025-5, EN 10155, EN 10025-1 | Strip, Sheet, Flat, Rod, Wire, Bar | |
300 °C | 1.36e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 1.36e-05 1/K | normalized or normalized formed (+N) | EN 10025-5, EN 10155, EN 10025-1 | Strip, Sheet, Flat, Rod, Wire, Bar | |
400 °C | 1.41e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 1.41e-05 1/K | normalized or normalized formed (+N) | EN 10025-5, EN 10155, EN 10025-1 | Strip, Sheet, Flat, Rod, Wire, Bar | |
500 °C | 1.45e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 1.45e-05 1/K | normalized or normalized formed (+N) | EN 10025-5, EN 10155, EN 10025-1 | Strip, Sheet, Flat, Rod, Wire, Bar | |
600 °C | 1.49e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 1.49e-05 1/K | normalized or normalized formed (+N) | EN 10025-5, EN 10155, EN 10025-1 | Strip, Sheet, Flat, Rod, Wire, Bar | |
Conductividad térmica | 20 °C | 56.9 W/(m·K) Show Material materials with Conductividad térmica of 56.9 W/(m·K) | normalized or normalized formed (+N) | EN 10025-5, EN 10155, EN 10025-1 | Strip, Sheet, Flat, Rod, Wire, Bar |
100 °C | 56.4 W/(m·K) Show Material materials with Conductividad térmica of 56.4 W/(m·K) | normalized or normalized formed (+N) | EN 10025-5, EN 10155, EN 10025-1 | Strip, Sheet, Flat, Rod, Wire, Bar | |
200 °C | 53.5 W/(m·K) Show Material materials with Conductividad térmica of 53.5 W/(m·K) | normalized or normalized formed (+N) | EN 10025-5, EN 10155, EN 10025-1 | Strip, Sheet, Flat, Rod, Wire, Bar | |
300 °C | 49.4 W/(m·K) Show Material materials with Conductividad térmica of 49.4 W/(m·K) | normalized or normalized formed (+N) | EN 10025-5, EN 10155, EN 10025-1 | Strip, Sheet, Flat, Rod, Wire, Bar | |
400 °C | 45.2 W/(m·K) Show Material materials with Conductividad térmica of 45.2 W/(m·K) | normalized or normalized formed (+N) | EN 10025-5, EN 10155, EN 10025-1 | Strip, Sheet, Flat, Rod, Wire, Bar | |
500 °C | 41.3 W/(m·K) Show Material materials with Conductividad térmica of 41.3 W/(m·K) | normalized or normalized formed (+N) | EN 10025-5, EN 10155, EN 10025-1 | Strip, Sheet, Flat, Rod, Wire, Bar | |
600 °C | 37.6 W/(m·K) Show Material materials with Conductividad térmica of 37.6 W/(m·K) | normalized or normalized formed (+N) | EN 10025-5, EN 10155, EN 10025-1 | Strip, Sheet, Flat, Rod, Wire, Bar | |
Difusividad térmica | 20 °C | 15.7 mm²/s Show Material materials with Difusividad térmica of 15.7 mm²/s | normalized or normalized formed (+N) | EN 10025-5, EN 10155, EN 10025-1 | Strip, Sheet, Flat, Rod, Wire, Bar |
100 °C | 14.5 mm²/s Show Material materials with Difusividad térmica of 14.5 mm²/s | normalized or normalized formed (+N) | EN 10025-5, EN 10155, EN 10025-1 | Strip, Sheet, Flat, Rod, Wire, Bar | |
200 °C | 12.9 mm²/s Show Material materials with Difusividad térmica of 12.9 mm²/s | normalized or normalized formed (+N) | EN 10025-5, EN 10155, EN 10025-1 | Strip, Sheet, Flat, Rod, Wire, Bar | |
300 °C | 11.2 mm²/s Show Material materials with Difusividad térmica of 11.2 mm²/s | normalized or normalized formed (+N) | EN 10025-5, EN 10155, EN 10025-1 | Strip, Sheet, Flat, Rod, Wire, Bar | |
400 °C | 9.6 mm²/s Show Material materials with Difusividad térmica of 9.6 mm²/s | normalized or normalized formed (+N) | EN 10025-5, EN 10155, EN 10025-1 | Strip, Sheet, Flat, Rod, Wire, Bar | |
500 °C | 7.9 mm²/s Show Material materials with Difusividad térmica of 7.9 mm²/s | normalized or normalized formed (+N) | EN 10025-5, EN 10155, EN 10025-1 | Strip, Sheet, Flat, Rod, Wire, Bar | |
600 °C | 6.3 mm²/s Show Material materials with Difusividad térmica of 6.3 mm²/s | normalized or normalized formed (+N) | EN 10025-5, EN 10155, EN 10025-1 | Strip, Sheet, Flat, Rod, Wire, Bar |
Eléctrico
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Resistividad eléctrica | 20 °C | 1.83e-07 Ω·m Show Material materials with Resistividad eléctrica of 1.83e-07 Ω·m | normalized or normalized formed (+N) | EN 10025-5, EN 10155, EN 10025-1 | Strip, Sheet, Flat, Rod, Wire, Bar |
100 °C | 2.27e-07 Ω·m Show Material materials with Resistividad eléctrica of 2.27e-07 Ω·m | normalized or normalized formed (+N) | EN 10025-5, EN 10155, EN 10025-1 | Strip, Sheet, Flat, Rod, Wire, Bar | |
200 °C | 2.95e-07 Ω·m Show Material materials with Resistividad eléctrica of 2.95e-07 Ω·m | normalized or normalized formed (+N) | EN 10025-5, EN 10155, EN 10025-1 | Strip, Sheet, Flat, Rod, Wire, Bar | |
300 °C | 3.8e-07 Ω·m Show Material materials with Resistividad eléctrica of 3.8e-07 Ω·m | normalized or normalized formed (+N) | EN 10025-5, EN 10155, EN 10025-1 | Strip, Sheet, Flat, Rod, Wire, Bar | |
400 °C | 4.81e-07 Ω·m Show Material materials with Resistividad eléctrica of 4.81e-07 Ω·m | normalized or normalized formed (+N) | EN 10025-5, EN 10155, EN 10025-1 | Strip, Sheet, Flat, Rod, Wire, Bar | |
500 °C | 5.99e-07 Ω·m Show Material materials with Resistividad eléctrica of 5.99e-07 Ω·m | normalized or normalized formed (+N) | EN 10025-5, EN 10155, EN 10025-1 | Strip, Sheet, Flat, Rod, Wire, Bar | |
600 °C | 7.38e-07 Ω·m Show Material materials with Resistividad eléctrica of 7.38e-07 Ω·m | normalized or normalized formed (+N) | EN 10025-5, EN 10155, EN 10025-1 | Strip, Sheet, Flat, Rod, Wire, Bar |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Azufre | 0.03 % Show Material materials with Azufre of 0.03 % | normalized or normalized formed (+N) | EN 10025-5, EN 10155 | Strip, Sheet, Flat, Rod, Wire |
0.035 % Show Material materials with Azufre of 0.035 % | normalized or normalized formed (+N) | EN 10155, EN 10025-1, EN 10025-5 | Bar, Sheet, Strip, Flat | |
Carbono | 0.13 % Show Material materials with Carbono of 0.13 % | normalized or normalized formed (+N) | EN 10025-5, EN 10155, EN 10025-1 | Strip, Sheet, Flat, Rod, Wire, Bar |
Cobre | 0.25 - 0.55 % Show Material materials with Cobre of 0.25 - 0.55 % | normalized or normalized formed (+N) | EN 10025-5, EN 10155, EN 10025-1 | Strip, Sheet, Flat, Rod, Wire, Bar |
Cromo | 0.4 - 0.8 % Show Material materials with Cromo of 0.4 - 0.8 % | normalized or normalized formed (+N) | EN 10025-5, EN 10155, EN 10025-1 | Strip, Sheet, Flat, Rod, Wire, Bar |
Fósforo | 0.035 % Show Material materials with Fósforo of 0.035 % | normalized or normalized formed (+N) | EN 10025-5, EN 10155 | Strip, Sheet, Flat, Rod, Wire |
0.04 % Show Material materials with Fósforo of 0.04 % | normalized or normalized formed (+N) | EN 10155, EN 10025-1, EN 10025-5 | Bar, Sheet, Strip, Flat | |
Manganeso | 0.2 - 0.8 % Show Material materials with Manganeso of 0.2 - 0.8 % | normalized or normalized formed (+N) | EN 10025-5, EN 10155, EN 10025-1 | Strip, Sheet, Flat, Rod, Wire, Bar |
Níquel | 0.65 % Show Material materials with Níquel of 0.65 % | normalized or normalized formed (+N) | EN 10025-5, EN 10155, EN 10025-1 | Strip, Sheet, Flat, Rod, Wire, Bar |
Silicona | 0.4 % Show Material materials with Silicona of 0.4 % | normalized or normalized formed (+N) | EN 10025-5, EN 10155, EN 10025-1 | Strip, Sheet, Flat, Rod, Wire, Bar |