General
Property | Temperature | Value |
---|---|---|
Densidad | 20.0 °C | 7.9 - 7.93 g/cm³ Show Material materials with Densidad of 7.9 - 7.93 g/cm³ |
Mecánica
Property | Temperature | Value | Comment |
---|---|---|---|
Coeficiente de Poisson | 23.0 °C | 0.3 [-] Show Material materials with Coeficiente de Poisson of 0.3 [-] | Typical for Austenitic Stainless Steel |
Elongación | -196.0 °C | 35 % Show Material materials with Elongación of 35 % | |
-150.0 °C | 35 % Show Material materials with Elongación of 35 % | ||
-80.0 °C | 40 % Show Material materials with Elongación of 40 % | ||
20.0 °C | 40 % Show Material materials with Elongación of 40 % | ||
Elongación A80 | 20.0 °C | 40 % Show Material materials with Elongación A80 of 40 % | |
Elongación A80 transversal | 20.0 °C | 40 % Show Material materials with Elongación A80 transversal of 40 % | |
Elongación transversal | 20.0 °C | 40 % Show Material materials with Elongación transversal of 40 % | |
Límite elástico Rp 0,2 | -196.0 °C | 550 MPa Show Material materials with Límite elástico Rp 0,2 of 550 MPa | |
-150.0 °C | 450 MPa Show Material materials with Límite elástico Rp 0,2 of 450 MPa | ||
-80.0 °C | 350 MPa Show Material materials with Límite elástico Rp 0,2 of 350 MPa | ||
20.0 °C | 270 - 290 MPa Show Material materials with Límite elástico Rp 0,2 of 270 - 290 MPa | ||
50.0 °C | 246 MPa Show Material materials with Límite elástico Rp 0,2 of 246 MPa | ||
100.0 °C | 205 MPa Show Material materials with Límite elástico Rp 0,2 of 205 MPa | ||
150.0 °C | 175 MPa Show Material materials with Límite elástico Rp 0,2 of 175 MPa | ||
200.0 °C | 157 MPa Show Material materials with Límite elástico Rp 0,2 of 157 MPa | ||
250.0 °C | 145 MPa Show Material materials with Límite elástico Rp 0,2 of 145 MPa | ||
300.0 °C | 136 MPa Show Material materials with Límite elástico Rp 0,2 of 136 MPa | ||
350.0 °C | 130 MPa Show Material materials with Límite elástico Rp 0,2 of 130 MPa | ||
400.0 °C | 125 MPa Show Material materials with Límite elástico Rp 0,2 of 125 MPa | ||
450.0 °C | 121 MPa Show Material materials with Límite elástico Rp 0,2 of 121 MPa | ||
500.0 °C | 119 MPa Show Material materials with Límite elástico Rp 0,2 of 119 MPa | ||
550.0 °C | 118 MPa Show Material materials with Límite elástico Rp 0,2 of 118 MPa | ||
Límite elástico Rp 1,0 | -196.0 °C | 650 MPa Show Material materials with Límite elástico Rp 1,0 of 650 MPa | |
-150.0 °C | 550 MPa Show Material materials with Límite elástico Rp 1,0 of 550 MPa | ||
-80.0 °C | 420 MPa Show Material materials with Límite elástico Rp 1,0 of 420 MPa | ||
20.0 °C | 310 - 320 MPa Show Material materials with Límite elástico Rp 1,0 of 310 - 320 MPa | ||
50.0 °C | 284 MPa Show Material materials with Límite elástico Rp 1,0 of 284 MPa | ||
100.0 °C | 240 MPa Show Material materials with Límite elástico Rp 1,0 of 240 MPa | ||
150.0 °C | 210 MPa Show Material materials with Límite elástico Rp 1,0 of 210 MPa | ||
200.0 °C | 187 MPa Show Material materials with Límite elástico Rp 1,0 of 187 MPa | ||
250.0 °C | 175 MPa Show Material materials with Límite elástico Rp 1,0 of 175 MPa | ||
300.0 °C | 167 MPa Show Material materials with Límite elástico Rp 1,0 of 167 MPa | ||
350.0 °C | 161 MPa Show Material materials with Límite elástico Rp 1,0 of 161 MPa | ||
400.0 °C | 156 MPa Show Material materials with Límite elástico Rp 1,0 of 156 MPa | ||
450.0 °C | 152 MPa Show Material materials with Límite elástico Rp 1,0 of 152 MPa | ||
500.0 °C | 149 MPa Show Material materials with Límite elástico Rp 1,0 of 149 MPa | ||
550.0 °C | 147 MPa Show Material materials with Límite elástico Rp 1,0 of 147 MPa | ||
Límite elástico transversal Rp 0,2 | 20.0 °C | 270 - 290 MPa Show Material materials with Límite elástico transversal Rp 0,2 of 270 - 290 MPa | |
Límite elástico transversal Rp 1,0 | 20.0 °C | 310 - 320 MPa Show Material materials with Límite elástico transversal Rp 1,0 of 310 - 320 MPa | |
Módulo de cizallamiento | 23.0 °C | 77 GPa Show Material materials with Módulo de cizallamiento of 77 GPa | Typical for Austenitic Stainless Steel |
Módulo elástico | -100.0 °C | 206 GPa Show Material materials with Módulo elástico of 206 GPa | |
20.0 °C | 196 - 200 GPa Show Material materials with Módulo elástico of 196 - 200 GPa | ||
100.0 °C | 190 - 194 GPa Show Material materials with Módulo elástico of 190 - 194 GPa | ||
200.0 °C | 182 - 186 GPa Show Material materials with Módulo elástico of 182 - 186 GPa | ||
300.0 °C | 174 - 179 GPa Show Material materials with Módulo elástico of 174 - 179 GPa | ||
400.0 °C | 166 - 172 GPa Show Material materials with Módulo elástico of 166 - 172 GPa | ||
500.0 °C | 158 - 165 GPa Show Material materials with Módulo elástico of 158 - 165 GPa | ||
600.0 °C | 150 GPa Show Material materials with Módulo elástico of 150 GPa | ||
700.0 °C | 142 GPa Show Material materials with Módulo elástico of 142 GPa | ||
800.0 °C | 134 GPa Show Material materials with Módulo elástico of 134 GPa | ||
900.0 °C | 127 GPa Show Material materials with Módulo elástico of 127 GPa | ||
1000.0 °C | 120 GPa Show Material materials with Módulo elástico of 120 GPa | ||
Resistencia a la tracción | -196.0 °C | 1250 MPa Show Material materials with Resistencia a la tracción of 1250 MPa | |
-150.0 °C | 1050 MPa Show Material materials with Resistencia a la tracción of 1050 MPa | ||
-80.0 °C | 850 MPa Show Material materials with Resistencia a la tracción of 850 MPa | ||
20.0 °C | 550 - 750 MPa Show Material materials with Resistencia a la tracción of 550 - 750 MPa | ||
50.0 °C | 527 MPa Show Material materials with Resistencia a la tracción of 527 MPa | ||
100.0 °C | 490 MPa Show Material materials with Resistencia a la tracción of 490 MPa | ||
150.0 °C | 460 MPa Show Material materials with Resistencia a la tracción of 460 MPa | ||
200.0 °C | 430 MPa Show Material materials with Resistencia a la tracción of 430 MPa | ||
250.0 °C | 420 MPa Show Material materials with Resistencia a la tracción of 420 MPa | ||
300.0 °C | 410 MPa Show Material materials with Resistencia a la tracción of 410 MPa | ||
350.0 °C | 410 MPa Show Material materials with Resistencia a la tracción of 410 MPa | ||
Resistencia a la tracción transversal | 20.0 °C | 550 - 750 MPa Show Material materials with Resistencia a la tracción transversal of 550 - 750 MPa |
Aplicaciones térmicas
Property | Temperature | Value | Comment |
---|---|---|---|
Calor específico | -100.0 °C | 440 J/(kg·K) Show Material materials with Calor específico of 440 J/(kg·K) | |
20.0 °C | 472 - 500 J/(kg·K) Show Material materials with Calor específico of 472 - 500 J/(kg·K) | ||
100.0 °C | 487 J/(kg·K) Show Material materials with Calor específico of 487 J/(kg·K) | ||
200.0 °C | 503 J/(kg·K) Show Material materials with Calor específico of 503 J/(kg·K) | ||
300.0 °C | 512 J/(kg·K) Show Material materials with Calor específico of 512 J/(kg·K) | ||
400.0 °C | 520 J/(kg·K) Show Material materials with Calor específico of 520 J/(kg·K) | ||
500.0 °C | 530 J/(kg·K) Show Material materials with Calor específico of 530 J/(kg·K) | ||
600.0 °C | 541 J/(kg·K) Show Material materials with Calor específico of 541 J/(kg·K) | ||
700.0 °C | 551 J/(kg·K) Show Material materials with Calor específico of 551 J/(kg·K) | ||
800.0 °C | 559 J/(kg·K) Show Material materials with Calor específico of 559 J/(kg·K) | ||
900.0 °C | 565 J/(kg·K) Show Material materials with Calor específico of 565 J/(kg·K) | ||
1000.0 °C | 571 J/(kg·K) Show Material materials with Calor específico of 571 J/(kg·K) | ||
Coeficiente de dilatación térmica | -100.0 °C | 1.49E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.49E-5 1/K | |
20.0 °C | 1.61E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.61E-5 1/K | ||
100.0 °C | 1.6E-5 - 1.67E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.6E-5 - 1.67E-5 1/K | ||
200.0 °C | 1.65E-5 - 1.72E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.65E-5 - 1.72E-5 1/K | ||
300.0 °C | 1.7E-5 - 1.77E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.7E-5 - 1.77E-5 1/K | ||
400.0 °C | 1.75E-5 - 1.81E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.75E-5 - 1.81E-5 1/K | ||
500.0 °C | 1.8E-5 - 1.84E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.8E-5 - 1.84E-5 1/K | ||
600.0 °C | 1.88E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.88E-5 1/K | ||
700.0 °C | 1.91E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.91E-5 1/K | ||
800.0 °C | 1.94E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.94E-5 1/K | ||
900.0 °C | 1.97E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.97E-5 1/K | ||
1000.0 °C | 2E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 2E-5 1/K | ||
Conductividad térmica | 20.0 °C | 14.3 - 15 W/(m·K) Show Material materials with Conductividad térmica of 14.3 - 15 W/(m·K) | |
100.0 °C | 15.8 W/(m·K) Show Material materials with Conductividad térmica of 15.8 W/(m·K) | ||
200.0 °C | 17.5 W/(m·K) Show Material materials with Conductividad térmica of 17.5 W/(m·K) | ||
300.0 °C | 19 W/(m·K) Show Material materials with Conductividad térmica of 19 W/(m·K) | ||
400.0 °C | 20.5 W/(m·K) Show Material materials with Conductividad térmica of 20.5 W/(m·K) | ||
500.0 °C | 21.9 W/(m·K) Show Material materials with Conductividad térmica of 21.9 W/(m·K) | ||
600.0 °C | 23.3 W/(m·K) Show Material materials with Conductividad térmica of 23.3 W/(m·K) | ||
700.0 °C | 24.6 W/(m·K) Show Material materials with Conductividad térmica of 24.6 W/(m·K) | ||
800.0 °C | 26 W/(m·K) Show Material materials with Conductividad térmica of 26 W/(m·K) | ||
900.0 °C | 27.4 W/(m·K) Show Material materials with Conductividad térmica of 27.4 W/(m·K) | ||
1000.0 °C | 28.8 W/(m·K) Show Material materials with Conductividad térmica of 28.8 W/(m·K) | ||
Difusividad térmica | 20.0 °C | 3.8 mm²/s Show Material materials with Difusividad térmica of 3.8 mm²/s | |
100.0 °C | 4 mm²/s Show Material materials with Difusividad térmica of 4 mm²/s | ||
200.0 °C | 4.2 mm²/s Show Material materials with Difusividad térmica of 4.2 mm²/s | ||
300.0 °C | 4.6 mm²/s Show Material materials with Difusividad térmica of 4.6 mm²/s | ||
400.0 °C | 4.8 mm²/s Show Material materials with Difusividad térmica of 4.8 mm²/s | ||
500.0 °C | 4.9 mm²/s Show Material materials with Difusividad térmica of 4.9 mm²/s | ||
600.0 °C | 5 mm²/s Show Material materials with Difusividad térmica of 5 mm²/s | ||
700.0 °C | 5.3 mm²/s Show Material materials with Difusividad térmica of 5.3 mm²/s | ||
800.0 °C | 5.6 mm²/s Show Material materials with Difusividad térmica of 5.6 mm²/s | ||
900.0 °C | 5.9 mm²/s Show Material materials with Difusividad térmica of 5.9 mm²/s | ||
1000.0 °C | 6 mm²/s Show Material materials with Difusividad térmica of 6 mm²/s | ||
Temperatura de fusión | 1230 - 1480 °C Show Material materials with Temperatura de fusión of 1230 - 1480 °C | Typical for Austenitic Stainless Steel | |
Temperatura máx. de funcionamiento, largo | -270 - 300 °C Show Material materials with Temperatura máx. de funcionamiento, largo of -270 - 300 °C |
Eléctrico
Property | Temperature | Value |
---|---|---|
Resistividad eléctrica | 20.0 °C | 7.1E-7 - 7.3E-7 Ω·m Show Material materials with Resistividad eléctrica of 7.1E-7 - 7.3E-7 Ω·m |
100.0 °C | 7.76E-7 Ω·m Show Material materials with Resistividad eléctrica of 7.76E-7 Ω·m | |
200.0 °C | 8.49E-7 Ω·m Show Material materials with Resistividad eléctrica of 8.49E-7 Ω·m | |
300.0 °C | 9.14E-7 Ω·m Show Material materials with Resistividad eléctrica of 9.14E-7 Ω·m | |
400.0 °C | 9.71E-7 Ω·m Show Material materials with Resistividad eléctrica of 9.71E-7 Ω·m | |
500.0 °C | 1.02E-6 Ω·m Show Material materials with Resistividad eléctrica of 1.02E-6 Ω·m | |
600.0 °C | 1.07E-6 Ω·m Show Material materials with Resistividad eléctrica of 1.07E-6 Ω·m | |
700.0 °C | 1.1E-6 Ω·m Show Material materials with Resistividad eléctrica of 1.1E-6 Ω·m | |
800.0 °C | 1.14E-6 Ω·m Show Material materials with Resistividad eléctrica of 1.14E-6 Ω·m | |
900.0 °C | 1.17E-6 Ω·m Show Material materials with Resistividad eléctrica of 1.17E-6 Ω·m | |
1000.0 °C | 1.19E-6 Ω·m Show Material materials with Resistividad eléctrica of 1.19E-6 Ω·m | |
Chemical properties
Property | Value |
---|---|
Azufre | 0.015 % Show Material materials with Azufre of 0.015 % |
Carbono | 0.03 % Show Material materials with Carbono of 0.03 % |
Cromo | 17 - 19.5 % Show Material materials with Cromo of 17 - 19.5 % |
Fósforo | 0.05 % Show Material materials with Fósforo of 0.05 % |
Manganeso | 2 % Show Material materials with Manganeso of 2 % |
Nitrógeno | 0.12 - 0.22 % Show Material materials with Nitrógeno of 0.12 - 0.22 % |
Níquel | 8.5 - 11.5 % Show Material materials with Níquel of 8.5 - 11.5 % |
Silicona | 1 % Show Material materials with Silicona of 1 % |