General
Property | Temperature | Value |
---|---|---|
Densidad | 20.0 °C | 7.96 - 8 g/cm³ Show Material materials with Densidad of 7.96 - 8 g/cm³ |
Mecánica
Property | Temperature | Value | Comment |
---|---|---|---|
Coeficiente de Poisson | 23.0 °C | 0.3 [-] Show Material materials with Coeficiente de Poisson of 0.3 [-] | Typical for Austenitic Stainless Steel |
Elongación | -196.0 °C | 35 % Show Material materials with Elongación of 35 % | |
-150.0 °C | 40 % Show Material materials with Elongación of 40 % | ||
-80.0 °C | 40 % Show Material materials with Elongación of 40 % | ||
20.0 °C | 45 % Show Material materials with Elongación of 45 % | ||
Elongación A80 transversal | 20.0 °C | 40 - 45 % Show Material materials with Elongación A80 transversal of 40 - 45 % | |
Elongación transversal | 20.0 °C | 40 - 45 % Show Material materials with Elongación transversal of 40 - 45 % | |
Límite elástico Rp 0,2 | -196.0 °C | 350 MPa Show Material materials with Límite elástico Rp 0,2 of 350 MPa | |
-150.0 °C | 315 MPa Show Material materials with Límite elástico Rp 0,2 of 315 MPa | ||
-80.0 °C | 275 MPa Show Material materials with Límite elástico Rp 0,2 of 275 MPa | ||
20.0 °C | 220 MPa Show Material materials with Límite elástico Rp 0,2 of 220 MPa | ||
50.0 °C | 200 MPa Show Material materials with Límite elástico Rp 0,2 of 200 MPa | ||
100.0 °C | 166 MPa Show Material materials with Límite elástico Rp 0,2 of 166 MPa | ||
150.0 °C | 152 MPa Show Material materials with Límite elástico Rp 0,2 of 152 MPa | ||
200.0 °C | 137 MPa Show Material materials with Límite elástico Rp 0,2 of 137 MPa | ||
250.0 °C | 127 MPa Show Material materials with Límite elástico Rp 0,2 of 127 MPa | ||
300.0 °C | 118 MPa Show Material materials with Límite elástico Rp 0,2 of 118 MPa | ||
350.0 °C | 113 MPa Show Material materials with Límite elástico Rp 0,2 of 113 MPa | ||
400.0 °C | 108 MPa Show Material materials with Límite elástico Rp 0,2 of 108 MPa | ||
450.0 °C | 103 MPa Show Material materials with Límite elástico Rp 0,2 of 103 MPa | ||
500.0 °C | 100 MPa Show Material materials with Límite elástico Rp 0,2 of 100 MPa | ||
550.0 °C | 98 MPa Show Material materials with Límite elástico Rp 0,2 of 98 MPa | ||
Límite elástico Rp 1,0 | -196.0 °C | 450 MPa Show Material materials with Límite elástico Rp 1,0 of 450 MPa | |
-150.0 °C | 415 MPa Show Material materials with Límite elástico Rp 1,0 of 415 MPa | ||
-80.0 °C | 355 MPa Show Material materials with Límite elástico Rp 1,0 of 355 MPa | ||
20.0 °C | 260 MPa Show Material materials with Límite elástico Rp 1,0 of 260 MPa | ||
50.0 °C | 237 MPa Show Material materials with Límite elástico Rp 1,0 of 237 MPa | ||
100.0 °C | 199 MPa Show Material materials with Límite elástico Rp 1,0 of 199 MPa | ||
150.0 °C | 181 MPa Show Material materials with Límite elástico Rp 1,0 of 181 MPa | ||
200.0 °C | 167 MPa Show Material materials with Límite elástico Rp 1,0 of 167 MPa | ||
250.0 °C | 157 MPa Show Material materials with Límite elástico Rp 1,0 of 157 MPa | ||
300.0 °C | 145 MPa Show Material materials with Límite elástico Rp 1,0 of 145 MPa | ||
350.0 °C | 139 MPa Show Material materials with Límite elástico Rp 1,0 of 139 MPa | ||
400.0 °C | 135 MPa Show Material materials with Límite elástico Rp 1,0 of 135 MPa | ||
450.0 °C | 130 MPa Show Material materials with Límite elástico Rp 1,0 of 130 MPa | ||
500.0 °C | 128 MPa Show Material materials with Límite elástico Rp 1,0 of 128 MPa | ||
550.0 °C | 127 MPa Show Material materials with Límite elástico Rp 1,0 of 127 MPa | ||
Límite elástico transversal Rp 0,2 | 20.0 °C | 220 - 240 MPa Show Material materials with Límite elástico transversal Rp 0,2 of 220 - 240 MPa | |
Límite elástico transversal Rp 1,0 | 20.0 °C | 260 - 270 MPa Show Material materials with Límite elástico transversal Rp 1,0 of 260 - 270 MPa | |
Módulo de cizallamiento | 23.0 °C | 77 GPa Show Material materials with Módulo de cizallamiento of 77 GPa | Typical for Austenitic Stainless Steel |
Módulo elástico | -100.0 °C | 206 GPa Show Material materials with Módulo elástico of 206 GPa | |
20.0 °C | 196 - 200 GPa Show Material materials with Módulo elástico of 196 - 200 GPa | ||
100.0 °C | 190 - 194 GPa Show Material materials with Módulo elástico of 190 - 194 GPa | ||
200.0 °C | 182 - 186 GPa Show Material materials with Módulo elástico of 182 - 186 GPa | ||
300.0 °C | 174 - 179 GPa Show Material materials with Módulo elástico of 174 - 179 GPa | ||
400.0 °C | 166 - 172 GPa Show Material materials with Módulo elástico of 166 - 172 GPa | ||
500.0 °C | 158 - 165 GPa Show Material materials with Módulo elástico of 158 - 165 GPa | ||
600.0 °C | 150 GPa Show Material materials with Módulo elástico of 150 GPa | ||
700.0 °C | 142 GPa Show Material materials with Módulo elástico of 142 GPa | ||
800.0 °C | 134 GPa Show Material materials with Módulo elástico of 134 GPa | ||
900.0 °C | 127 GPa Show Material materials with Módulo elástico of 127 GPa | ||
1000.0 °C | 120 GPa Show Material materials with Módulo elástico of 120 GPa | ||
Resistencia a la tracción | -196.0 °C | 1200 MPa Show Material materials with Resistencia a la tracción of 1200 MPa | |
-150.0 °C | 1070 MPa Show Material materials with Resistencia a la tracción of 1070 MPa | ||
-80.0 °C | 840 MPa Show Material materials with Resistencia a la tracción of 840 MPa | ||
20.0 °C | 520 - 680 MPa Show Material materials with Resistencia a la tracción of 520 - 680 MPa | ||
50.0 °C | 486 MPa Show Material materials with Resistencia a la tracción of 486 MPa | ||
100.0 °C | 430 MPa Show Material materials with Resistencia a la tracción of 430 MPa | ||
150.0 °C | 410 MPa Show Material materials with Resistencia a la tracción of 410 MPa | ||
200.0 °C | 390 MPa Show Material materials with Resistencia a la tracción of 390 MPa | ||
250.0 °C | 385 MPa Show Material materials with Resistencia a la tracción of 385 MPa | ||
300.0 °C | 380 MPa Show Material materials with Resistencia a la tracción of 380 MPa | ||
350.0 °C | 380 MPa Show Material materials with Resistencia a la tracción of 380 MPa | ||
400.0 °C | 380 MPa Show Material materials with Resistencia a la tracción of 380 MPa | ||
500.0 °C | 360 MPa Show Material materials with Resistencia a la tracción of 360 MPa | ||
Resistencia a la tracción transversal | 20.0 °C | 520 - 680 MPa Show Material materials with Resistencia a la tracción transversal of 520 - 680 MPa |
Aplicaciones térmicas
Property | Temperature | Value | Comment |
---|---|---|---|
Calor específico | -100.0 °C | 440 J/(kg·K) Show Material materials with Calor específico of 440 J/(kg·K) | |
20.0 °C | 472 - 500 J/(kg·K) Show Material materials with Calor específico of 472 - 500 J/(kg·K) | ||
100.0 °C | 487 J/(kg·K) Show Material materials with Calor específico of 487 J/(kg·K) | ||
200.0 °C | 503 J/(kg·K) Show Material materials with Calor específico of 503 J/(kg·K) | ||
300.0 °C | 512 J/(kg·K) Show Material materials with Calor específico of 512 J/(kg·K) | ||
400.0 °C | 520 J/(kg·K) Show Material materials with Calor específico of 520 J/(kg·K) | ||
500.0 °C | 530 J/(kg·K) Show Material materials with Calor específico of 530 J/(kg·K) | ||
600.0 °C | 541 J/(kg·K) Show Material materials with Calor específico of 541 J/(kg·K) | ||
700.0 °C | 551 J/(kg·K) Show Material materials with Calor específico of 551 J/(kg·K) | ||
800.0 °C | 559 J/(kg·K) Show Material materials with Calor específico of 559 J/(kg·K) | ||
900.0 °C | 565 J/(kg·K) Show Material materials with Calor específico of 565 J/(kg·K) | ||
1000.0 °C | 571 J/(kg·K) Show Material materials with Calor específico of 571 J/(kg·K) | ||
Coeficiente de dilatación térmica | -100.0 °C | 1.49E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.49E-5 1/K | |
20.0 °C | 1.61E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.61E-5 1/K | ||
100.0 °C | 1.6E-5 - 1.67E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.6E-5 - 1.67E-5 1/K | ||
200.0 °C | 1.65E-5 - 1.72E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.65E-5 - 1.72E-5 1/K | ||
300.0 °C | 1.7E-5 - 1.77E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.7E-5 - 1.77E-5 1/K | ||
400.0 °C | 1.75E-5 - 1.81E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.75E-5 - 1.81E-5 1/K | ||
500.0 °C | 1.8E-5 - 1.84E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.8E-5 - 1.84E-5 1/K | ||
600.0 °C | 1.88E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.88E-5 1/K | ||
700.0 °C | 1.91E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.91E-5 1/K | ||
800.0 °C | 1.94E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.94E-5 1/K | ||
900.0 °C | 1.97E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.97E-5 1/K | ||
1000.0 °C | 2E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 2E-5 1/K | ||
Conductividad térmica | 20.0 °C | 13.3 - 15 W/(m·K) Show Material materials with Conductividad térmica of 13.3 - 15 W/(m·K) | |
100.0 °C | 14.9 W/(m·K) Show Material materials with Conductividad térmica of 14.9 W/(m·K) | ||
200.0 °C | 16.5 W/(m·K) Show Material materials with Conductividad térmica of 16.5 W/(m·K) | ||
300.0 °C | 18.1 W/(m·K) Show Material materials with Conductividad térmica of 18.1 W/(m·K) | ||
400.0 °C | 19.5 W/(m·K) Show Material materials with Conductividad térmica of 19.5 W/(m·K) | ||
500.0 °C | 21 W/(m·K) Show Material materials with Conductividad térmica of 21 W/(m·K) | ||
600.0 °C | 22.4 W/(m·K) Show Material materials with Conductividad térmica of 22.4 W/(m·K) | ||
700.0 °C | 23.8 W/(m·K) Show Material materials with Conductividad térmica of 23.8 W/(m·K) | ||
800.0 °C | 25.2 W/(m·K) Show Material materials with Conductividad térmica of 25.2 W/(m·K) | ||
Difusividad térmica | 20.0 °C | 3.5 mm²/s Show Material materials with Difusividad térmica of 3.5 mm²/s | |
100.0 °C | 3.8 mm²/s Show Material materials with Difusividad térmica of 3.8 mm²/s | ||
200.0 °C | 4 mm²/s Show Material materials with Difusividad térmica of 4 mm²/s | ||
300.0 °C | 4.3 mm²/s Show Material materials with Difusividad térmica of 4.3 mm²/s | ||
400.0 °C | 4.5 mm²/s Show Material materials with Difusividad térmica of 4.5 mm²/s | ||
500.0 °C | 4.7 mm²/s Show Material materials with Difusividad térmica of 4.7 mm²/s | ||
600.0 °C | 4.8 mm²/s Show Material materials with Difusividad térmica of 4.8 mm²/s | ||
700.0 °C | 5.1 mm²/s Show Material materials with Difusividad térmica of 5.1 mm²/s | ||
800.0 °C | 5.4 mm²/s Show Material materials with Difusividad térmica of 5.4 mm²/s | ||
Temperatura de fusión | 1230 - 1480 °C Show Material materials with Temperatura de fusión of 1230 - 1480 °C | Typical for Austenitic Stainless Steel | |
Temperatura máx. de funcionamiento, largo | 0 - 400 °C Show Material materials with Temperatura máx. de funcionamiento, largo of 0 - 400 °C |
Eléctrico
Property | Temperature | Value |
---|---|---|
Resistividad eléctrica | 20.0 °C | 7.5E-7 - 7.91E-7 Ω·m Show Material materials with Resistividad eléctrica of 7.5E-7 - 7.91E-7 Ω·m |
100.0 °C | 8.45E-7 Ω·m Show Material materials with Resistividad eléctrica of 8.45E-7 Ω·m | |
200.0 °C | 9.19E-7 Ω·m Show Material materials with Resistividad eléctrica of 9.19E-7 Ω·m | |
300.0 °C | 9.77E-7 Ω·m Show Material materials with Resistividad eléctrica of 9.77E-7 Ω·m | |
400.0 °C | 1.03E-6 Ω·m Show Material materials with Resistividad eléctrica of 1.03E-6 Ω·m | |
500.0 °C | 1.08E-6 Ω·m Show Material materials with Resistividad eléctrica of 1.08E-6 Ω·m | |
600.0 °C | 1.12E-6 Ω·m Show Material materials with Resistividad eléctrica of 1.12E-6 Ω·m | |
700.0 °C | 1.15E-6 Ω·m Show Material materials with Resistividad eléctrica of 1.15E-6 Ω·m | |
800.0 °C | 1.18E-6 Ω·m Show Material materials with Resistividad eléctrica of 1.18E-6 Ω·m | |
Chemical properties
Property | Value |
---|---|
Azufre | 0.015 % Show Material materials with Azufre of 0.015 % |
Carbono | 0.03 % Show Material materials with Carbono of 0.03 % |
Cromo | 16.5 - 18.5 % Show Material materials with Cromo of 16.5 - 18.5 % |
Fósforo | 0.05 % Show Material materials with Fósforo of 0.05 % |
Manganeso | 2 % Show Material materials with Manganeso of 2 % |
Molibdeno | 2 - 2.5 % Show Material materials with Molibdeno of 2 - 2.5 % |
Nitrógeno | 0.1 - 0.11 % Show Material materials with Nitrógeno of 0.1 - 0.11 % |
Níquel | 10 - 13 % Show Material materials with Níquel of 10 - 13 % |
Silicona | 1 % Show Material materials with Silicona of 1 % |