General
Property | Temperature | Value |
---|---|---|
Densidad | 20.0 °C | 7.94 - 8 g/cm³ Show Material materials with Densidad of 7.94 - 8 g/cm³ |
Mecánica
Property | Temperature | Value | Comment |
---|---|---|---|
Coeficiente de Poisson | 23.0 °C | 0.3 [-] Show Material materials with Coeficiente de Poisson of 0.3 [-] | Typical for Austenitic Stainless Steel |
Elongación A80 transversal | 20.0 °C | 30 % Show Material materials with Elongación A80 transversal of 30 % | |
Elongación transversal | 20.0 °C | 30 % Show Material materials with Elongación transversal of 30 % | |
Límite elástico Rp 0,2 | 50.0 °C | 159 MPa Show Material materials with Límite elástico Rp 0,2 of 159 MPa | |
100.0 °C | 140 MPa Show Material materials with Límite elástico Rp 0,2 of 140 MPa | ||
150.0 °C | 127 MPa Show Material materials with Límite elástico Rp 0,2 of 127 MPa | ||
200.0 °C | 115 MPa Show Material materials with Límite elástico Rp 0,2 of 115 MPa | ||
250.0 °C | 105 MPa Show Material materials with Límite elástico Rp 0,2 of 105 MPa | ||
300.0 °C | 95 MPa Show Material materials with Límite elástico Rp 0,2 of 95 MPa | ||
350.0 °C | 90 MPa Show Material materials with Límite elástico Rp 0,2 of 90 MPa | ||
400.0 °C | 85 MPa Show Material materials with Límite elástico Rp 0,2 of 85 MPa | ||
450.0 °C | 82 MPa Show Material materials with Límite elástico Rp 0,2 of 82 MPa | ||
500.0 °C | 80 MPa Show Material materials with Límite elástico Rp 0,2 of 80 MPa | ||
550.0 °C | 75 MPa Show Material materials with Límite elástico Rp 0,2 of 75 MPa | ||
600.0 °C | 75 MPa Show Material materials with Límite elástico Rp 0,2 of 75 MPa | ||
Límite elástico Rp 1,0 | 50.0 °C | 185 MPa Show Material materials with Límite elástico Rp 1,0 of 185 MPa | |
100.0 °C | 160 MPa Show Material materials with Límite elástico Rp 1,0 of 160 MPa | ||
150.0 °C | 147 MPa Show Material materials with Límite elástico Rp 1,0 of 147 MPa | ||
200.0 °C | 135 MPa Show Material materials with Límite elástico Rp 1,0 of 135 MPa | ||
250.0 °C | 125 MPa Show Material materials with Límite elástico Rp 1,0 of 125 MPa | ||
300.0 °C | 115 MPa Show Material materials with Límite elástico Rp 1,0 of 115 MPa | ||
350.0 °C | 110 MPa Show Material materials with Límite elástico Rp 1,0 of 110 MPa | ||
400.0 °C | 105 MPa Show Material materials with Límite elástico Rp 1,0 of 105 MPa | ||
450.0 °C | 102 MPa Show Material materials with Límite elástico Rp 1,0 of 102 MPa | ||
500.0 °C | 100 MPa Show Material materials with Límite elástico Rp 1,0 of 100 MPa | ||
550.0 °C | 95 MPa Show Material materials with Límite elástico Rp 1,0 of 95 MPa | ||
600.0 °C | 95 MPa Show Material materials with Límite elástico Rp 1,0 of 95 MPa | ||
Límite elástico transversal Rp 0,2 | 20.0 °C | 170 MPa Show Material materials with Límite elástico transversal Rp 0,2 of 170 MPa | |
Límite elástico transversal Rp 1,0 | 20.0 °C | 200 MPa Show Material materials with Límite elástico transversal Rp 1,0 of 200 MPa | |
Módulo de cizallamiento | 23.0 °C | 77 GPa Show Material materials with Módulo de cizallamiento of 77 GPa | Typical for Austenitic Stainless Steel |
Módulo elástico | -100.0 °C | 201 GPa Show Material materials with Módulo elástico of 201 GPa | |
20.0 °C | 194 - 200 GPa Show Material materials with Módulo elástico of 194 - 200 GPa | ||
100.0 °C | 189 - 190 GPa Show Material materials with Módulo elástico of 189 - 190 GPa | ||
200.0 °C | 183 - 185 GPa Show Material materials with Módulo elástico of 183 - 185 GPa | ||
300.0 °C | 175 - 177 GPa Show Material materials with Módulo elástico of 175 - 177 GPa | ||
400.0 °C | 170 GPa Show Material materials with Módulo elástico of 170 GPa | ||
500.0 °C | 160 - 163 GPa Show Material materials with Módulo elástico of 160 - 163 GPa | ||
600.0 °C | 155 - 156 GPa Show Material materials with Módulo elástico of 155 - 156 GPa | ||
700.0 °C | 145 - 149 GPa Show Material materials with Módulo elástico of 145 - 149 GPa | ||
800.0 °C | 140 - 141 GPa Show Material materials with Módulo elástico of 140 - 141 GPa | ||
900.0 °C | 134 - 135 GPa Show Material materials with Módulo elástico of 134 - 135 GPa | ||
1000.0 °C | 125 - 127 GPa Show Material materials with Módulo elástico of 125 - 127 GPa | ||
Resistencia a la tracción | 20.0 °C | 500 - 750 MPa Show Material materials with Resistencia a la tracción of 500 - 750 MPa | |
50.0 °C | 487 MPa Show Material materials with Resistencia a la tracción of 487 MPa | ||
100.0 °C | 465 MPa Show Material materials with Resistencia a la tracción of 465 MPa | ||
150.0 °C | 445 MPa Show Material materials with Resistencia a la tracción of 445 MPa | ||
200.0 °C | 435 MPa Show Material materials with Resistencia a la tracción of 435 MPa | ||
250.0 °C | 425 MPa Show Material materials with Resistencia a la tracción of 425 MPa | ||
300.0 °C | 420 MPa Show Material materials with Resistencia a la tracción of 420 MPa | ||
350.0 °C | 418 MPa Show Material materials with Resistencia a la tracción of 418 MPa | ||
400.0 °C | 415 MPa Show Material materials with Resistencia a la tracción of 415 MPa | ||
450.0 °C | 415 MPa Show Material materials with Resistencia a la tracción of 415 MPa | ||
500.0 °C | 415 MPa Show Material materials with Resistencia a la tracción of 415 MPa | ||
Resistencia a la tracción transversal | 20.0 °C | 500 - 750 MPa Show Material materials with Resistencia a la tracción transversal of 500 - 750 MPa |
Aplicaciones térmicas
Property | Temperature | Value | Comment |
---|---|---|---|
Calor específico | -100.0 °C | 440 J/(kg·K) Show Material materials with Calor específico of 440 J/(kg·K) | |
20.0 °C | 460 - 472 J/(kg·K) Show Material materials with Calor específico of 460 - 472 J/(kg·K) | ||
100.0 °C | 487 J/(kg·K) Show Material materials with Calor específico of 487 J/(kg·K) | ||
200.0 °C | 503 J/(kg·K) Show Material materials with Calor específico of 503 J/(kg·K) | ||
300.0 °C | 512 J/(kg·K) Show Material materials with Calor específico of 512 J/(kg·K) | ||
400.0 °C | 520 J/(kg·K) Show Material materials with Calor específico of 520 J/(kg·K) | ||
500.0 °C | 530 J/(kg·K) Show Material materials with Calor específico of 530 J/(kg·K) | ||
600.0 °C | 541 J/(kg·K) Show Material materials with Calor específico of 541 J/(kg·K) | ||
700.0 °C | 551 J/(kg·K) Show Material materials with Calor específico of 551 J/(kg·K) | ||
800.0 °C | 559 J/(kg·K) Show Material materials with Calor específico of 559 J/(kg·K) | ||
900.0 °C | 565 J/(kg·K) Show Material materials with Calor específico of 565 J/(kg·K) | ||
1000.0 °C | 571 J/(kg·K) Show Material materials with Calor específico of 571 J/(kg·K) | ||
Coeficiente de dilatación térmica | -100.0 °C | 1.36E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.36E-5 1/K | |
20.0 °C | 1.46E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.46E-5 1/K | ||
100.0 °C | 1.51E-5 - 1.54E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.51E-5 - 1.54E-5 1/K | ||
200.0 °C | 1.57E-5 - 1.6E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.57E-5 - 1.6E-5 1/K | ||
300.0 °C | 1.62E-5 - 1.65E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.62E-5 - 1.65E-5 1/K | ||
400.0 °C | 1.66E-5 - 1.68E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.66E-5 - 1.68E-5 1/K | ||
500.0 °C | 1.7E-5 - 1.72E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.7E-5 - 1.72E-5 1/K | ||
600.0 °C | 1.74E-5 - 1.75E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.74E-5 - 1.75E-5 1/K | ||
700.0 °C | 1.77E-5 - 1.79E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.77E-5 - 1.79E-5 1/K | ||
800.0 °C | 1.8E-5 - 1.83E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.8E-5 - 1.83E-5 1/K | ||
900.0 °C | 1.83E-5 - 1.86E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.83E-5 - 1.86E-5 1/K | ||
1000.0 °C | 1.86E-5 - 1.9E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.86E-5 - 1.9E-5 1/K | ||
Conductividad térmica | 20.0 °C | 11.5 - 12 W/(m·K) Show Material materials with Conductividad térmica of 11.5 - 12 W/(m·K) | |
100.0 °C | 13.1 W/(m·K) Show Material materials with Conductividad térmica of 13.1 W/(m·K) | ||
200.0 °C | 14.8 W/(m·K) Show Material materials with Conductividad térmica of 14.8 W/(m·K) | ||
300.0 °C | 16.4 W/(m·K) Show Material materials with Conductividad térmica of 16.4 W/(m·K) | ||
400.0 °C | 18.1 W/(m·K) Show Material materials with Conductividad térmica of 18.1 W/(m·K) | ||
500.0 °C | 19.6 W/(m·K) Show Material materials with Conductividad térmica of 19.6 W/(m·K) | ||
600.0 °C | 21.2 W/(m·K) Show Material materials with Conductividad térmica of 21.2 W/(m·K) | ||
700.0 °C | 22.8 W/(m·K) Show Material materials with Conductividad térmica of 22.8 W/(m·K) | ||
800.0 °C | 24.3 W/(m·K) Show Material materials with Conductividad térmica of 24.3 W/(m·K) | ||
900.0 °C | 25.7 W/(m·K) Show Material materials with Conductividad térmica of 25.7 W/(m·K) | ||
1000.0 °C | 27.3 W/(m·K) Show Material materials with Conductividad térmica of 27.3 W/(m·K) | ||
Difusividad térmica | 20.0 °C | 3.1 mm²/s Show Material materials with Difusividad térmica of 3.1 mm²/s | |
100.0 °C | 3.3 mm²/s Show Material materials with Difusividad térmica of 3.3 mm²/s | ||
200.0 °C | 3.6 mm²/s Show Material materials with Difusividad térmica of 3.6 mm²/s | ||
300.0 °C | 3.9 mm²/s Show Material materials with Difusividad térmica of 3.9 mm²/s | ||
400.0 °C | 4.2 mm²/s Show Material materials with Difusividad térmica of 4.2 mm²/s | ||
500.0 °C | 4.4 mm²/s Show Material materials with Difusividad térmica of 4.4 mm²/s | ||
600.0 °C | 4.6 mm²/s Show Material materials with Difusividad térmica of 4.6 mm²/s | ||
700.0 °C | 4.9 mm²/s Show Material materials with Difusividad térmica of 4.9 mm²/s | ||
800.0 °C | 5.2 mm²/s Show Material materials with Difusividad térmica of 5.2 mm²/s | ||
900.0 °C | 5.5 mm²/s Show Material materials with Difusividad térmica of 5.5 mm²/s | ||
1000.0 °C | 5.7 mm²/s Show Material materials with Difusividad térmica of 5.7 mm²/s | ||
Temperatura de fusión | 1230 - 1480 °C Show Material materials with Temperatura de fusión of 1230 - 1480 °C | Typical for Austenitic Stainless Steel | |
Temperatura máx. de funcionamiento, largo | 700 - 1000 °C Show Material materials with Temperatura máx. de funcionamiento, largo of 700 - 1000 °C |
Eléctrico
Property | Temperature | Value |
---|---|---|
Resistividad eléctrica | 20.0 °C | 9.9E-7 - 1.01E-6 Ω·m Show Material materials with Resistividad eléctrica of 9.9E-7 - 1.01E-6 Ω·m |
100.0 °C | 1.04E-6 Ω·m Show Material materials with Resistividad eléctrica of 1.04E-6 Ω·m | |
200.0 °C | 1.08E-6 Ω·m Show Material materials with Resistividad eléctrica of 1.08E-6 Ω·m | |
300.0 °C | 1.12E-6 Ω·m Show Material materials with Resistividad eléctrica of 1.12E-6 Ω·m | |
400.0 °C | 1.15E-6 Ω·m Show Material materials with Resistividad eléctrica of 1.15E-6 Ω·m | |
500.0 °C | 1.18E-6 Ω·m Show Material materials with Resistividad eléctrica of 1.18E-6 Ω·m | |
600.0 °C | 1.2E-6 Ω·m Show Material materials with Resistividad eléctrica of 1.2E-6 Ω·m | |
700.0 °C | 1.22E-6 Ω·m Show Material materials with Resistividad eléctrica of 1.22E-6 Ω·m | |
800.0 °C | 1.24E-6 Ω·m Show Material materials with Resistividad eléctrica of 1.24E-6 Ω·m | |
900.0 °C | 1.26E-6 Ω·m Show Material materials with Resistividad eléctrica of 1.26E-6 Ω·m | |
1000.0 °C | 1.27E-6 Ω·m Show Material materials with Resistividad eléctrica of 1.27E-6 Ω·m | |
Chemical properties
Property | Value |
---|---|
Aluminio | 0.25 - 0.65 % Show Material materials with Aluminio of 0.25 - 0.65 % |
Azufre | 0.01 % Show Material materials with Azufre of 0.01 % |
Carbono | 0.05 - 0.1 % Show Material materials with Carbono of 0.05 - 0.1 % |
Cobalto | 0.5 % Show Material materials with Cobalto of 0.5 % |
Cobre | 0.5 % Show Material materials with Cobre of 0.5 % |
Cromo | 19 - 22 % Show Material materials with Cromo of 19 - 22 % |
Fósforo | 0.02 % Show Material materials with Fósforo of 0.02 % |
Manganeso | 1.5 % Show Material materials with Manganeso of 1.5 % |
Nitrógeno | 0.03 % Show Material materials with Nitrógeno of 0.03 % |
Níquel | 30 - 34 % Show Material materials with Níquel of 30 - 34 % |
Silicona | 0.7 % Show Material materials with Silicona of 0.7 % |
Titanio | 0.25 - 0.65 % Show Material materials with Titanio of 0.25 - 0.65 % |