General
Property | Temperature | Value |
---|---|---|
Densidad | 20.0 °C | 7.86 g/cm³ Show Material materials with Densidad of 7.86 g/cm³ |
27.0 °C | 7.82 g/cm³ Show Material materials with Densidad of 7.82 g/cm³ | |
Mecánica
Property | Temperature | Value |
---|---|---|
Coeficiente de Poisson | -269.0 °C | 0.28 [-] Show Material materials with Coeficiente de Poisson of 0.28 [-] |
-200.0 °C | 0.28 [-] Show Material materials with Coeficiente de Poisson of 0.28 [-] | |
-150.0 °C | 0.28 [-] Show Material materials with Coeficiente de Poisson of 0.28 [-] | |
-100.0 °C | 0.28 [-] Show Material materials with Coeficiente de Poisson of 0.28 [-] | |
-50.0 °C | 0.29 [-] Show Material materials with Coeficiente de Poisson of 0.29 [-] | |
27.0 °C | 0.29 [-] Show Material materials with Coeficiente de Poisson of 0.29 [-] | |
Elongación | 20.0 °C | 19 % Show Material materials with Elongación of 19 % |
Límite elástico | 20.0 °C | 380 MPa Show Material materials with Límite elástico of 380 MPa |
Módulo de cizallamiento | -269.0 °C | 81.7 GPa Show Material materials with Módulo de cizallamiento of 81.7 GPa |
-200.0 °C | 81.8 GPa Show Material materials with Módulo de cizallamiento of 81.8 GPa | |
-150.0 °C | 81.1 GPa Show Material materials with Módulo de cizallamiento of 81.1 GPa | |
-100.0 °C | 80.2 GPa Show Material materials with Módulo de cizallamiento of 80.2 GPa | |
-50.0 °C | 79 GPa Show Material materials with Módulo de cizallamiento of 79 GPa | |
27.0 °C | 77 GPa Show Material materials with Módulo de cizallamiento of 77 GPa | |
Módulo elástico | -269.0 °C | 209.4 GPa Show Material materials with Módulo elástico of 209.4 GPa |
-200.0 °C | 209.5 GPa Show Material materials with Módulo elástico of 209.5 GPa | |
-150.0 °C | 208 GPa Show Material materials with Módulo elástico of 208 GPa | |
-100.0 °C | 205.9 - 210 GPa Show Material materials with Módulo elástico of 205.9 - 210 GPa | |
-50.0 °C | 203.1 GPa Show Material materials with Módulo elástico of 203.1 GPa | |
20.0 °C | 204 GPa Show Material materials with Módulo elástico of 204 GPa | |
27.0 °C | 198.4 GPa Show Material materials with Módulo elástico of 198.4 GPa | |
100.0 °C | 199 GPa Show Material materials with Módulo elástico of 199 GPa | |
200.0 °C | 193 GPa Show Material materials with Módulo elástico of 193 GPa | |
300.0 °C | 186 GPa Show Material materials with Módulo elástico of 186 GPa | |
400.0 °C | 178 GPa Show Material materials with Módulo elástico of 178 GPa | |
Resistencia a la tracción | 20.0 °C | 510 - 710 MPa Show Material materials with Resistencia a la tracción of 510 - 710 MPa |
Aplicaciones térmicas
Property | Temperature | Value | Comment |
---|---|---|---|
Calor específico | -100.0 °C | 440 J/(kg·K) Show Material materials with Calor específico of 440 J/(kg·K) | |
20.0 °C | 463 J/(kg·K) Show Material materials with Calor específico of 463 J/(kg·K) | ||
100.0 °C | 477 J/(kg·K) Show Material materials with Calor específico of 477 J/(kg·K) | ||
200.0 °C | 494 J/(kg·K) Show Material materials with Calor específico of 494 J/(kg·K) | ||
300.0 °C | 510 J/(kg·K) Show Material materials with Calor específico of 510 J/(kg·K) | ||
400.0 °C | 529 J/(kg·K) Show Material materials with Calor específico of 529 J/(kg·K) | ||
Coeficiente de dilatación térmica | -100.0 °C | 1.02E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.02E-5 1/K | |
20.0 °C | 1.12E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.12E-5 1/K | ||
100.0 °C | 1.17E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.17E-5 1/K | ||
200.0 °C | 1.21E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.21E-5 1/K | ||
300.0 °C | 1.25E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.25E-5 1/K | ||
400.0 °C | 1.28E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.28E-5 1/K | ||
Conductividad térmica | -100.0 °C | 29.5 W/(m·K) Show Material materials with Conductividad térmica of 29.5 W/(m·K) | |
20.0 °C | 36.2 W/(m·K) Show Material materials with Conductividad térmica of 36.2 W/(m·K) | ||
100.0 °C | 38.5 W/(m·K) Show Material materials with Conductividad térmica of 38.5 W/(m·K) | ||
200.0 °C | 39 W/(m·K) Show Material materials with Conductividad térmica of 39 W/(m·K) | ||
300.0 °C | 38.3 W/(m·K) Show Material materials with Conductividad térmica of 38.3 W/(m·K) | ||
400.0 °C | 36.2 W/(m·K) Show Material materials with Conductividad térmica of 36.2 W/(m·K) | ||
Difusividad térmica | 20.0 °C | 10 mm²/s Show Material materials with Difusividad térmica of 10 mm²/s | |
100.0 °C | 10 mm²/s Show Material materials with Difusividad térmica of 10 mm²/s | ||
200.0 °C | 9.6 mm²/s Show Material materials with Difusividad térmica of 9.6 mm²/s | ||
300.0 °C | 8.8 mm²/s Show Material materials with Difusividad térmica of 8.8 mm²/s | ||
400.0 °C | 7.7 mm²/s Show Material materials with Difusividad térmica of 7.7 mm²/s | ||
Temperatura de fusión | 1316 - 1595 °C Show Material materials with Temperatura de fusión of 1316 - 1595 °C | Typical for Nickel Steel |
Eléctrico
Property | Temperature | Value |
---|---|---|
Resistividad eléctrica | -100.0 °C | 1.95E-7 Ω·m Show Material materials with Resistividad eléctrica of 1.95E-7 Ω·m |
20.0 °C | 2.61E-7 Ω·m Show Material materials with Resistividad eléctrica of 2.61E-7 Ω·m | |
100.0 °C | 3.1E-7 Ω·m Show Material materials with Resistividad eléctrica of 3.1E-7 Ω·m | |
200.0 °C | 3.78E-7 Ω·m Show Material materials with Resistividad eléctrica of 3.78E-7 Ω·m | |
300.0 °C | 4.57E-7 Ω·m Show Material materials with Resistividad eléctrica of 4.57E-7 Ω·m | |
400.0 °C | 5.57E-7 Ω·m Show Material materials with Resistividad eléctrica of 5.57E-7 Ω·m | |
Chemical properties
Property | Value |
---|---|
Azufre | 5E-3 % Show Material materials with Azufre of 5E-3 % |
Carbono | 0.15 % Show Material materials with Carbono of 0.15 % |
Fósforo | 0.02 % Show Material materials with Fósforo of 0.02 % |
Manganeso | 0.3 - 0.8 % Show Material materials with Manganeso of 0.3 - 0.8 % |
Níquel | 4.75 - 5.25 % Show Material materials with Níquel of 4.75 - 5.25 % |
Silicona | 0.35 % Show Material materials with Silicona of 0.35 % |
Vanadio | 0.05 % Show Material materials with Vanadio of 0.05 % |