General
Property | Temperature | Value |
---|---|---|
Densidad | 20.0 °C | 7.88 g/cm³ Show Material materials with Densidad of 7.88 g/cm³ |
27.0 °C | 7.84 g/cm³ Show Material materials with Densidad of 7.84 g/cm³ | |
Mecánica
Property | Temperature | Value |
---|---|---|
Coeficiente de Poisson | -269.0 °C | 0.29 [-] Show Material materials with Coeficiente de Poisson of 0.29 [-] |
-200.0 °C | 0.29 [-] Show Material materials with Coeficiente de Poisson of 0.29 [-] | |
-150.0 °C | 0.29 [-] Show Material materials with Coeficiente de Poisson of 0.29 [-] | |
-100.0 °C | 0.29 [-] Show Material materials with Coeficiente de Poisson of 0.29 [-] | |
-50.0 °C | 0.29 [-] Show Material materials with Coeficiente de Poisson of 0.29 [-] | |
27.0 °C | 0.29 [-] Show Material materials with Coeficiente de Poisson of 0.29 [-] | |
Elongación | 20.0 °C | 18 % Show Material materials with Elongación of 18 % |
Límite elástico | 20.0 °C | 480 - 490 MPa Show Material materials with Límite elástico of 480 - 490 MPa |
Módulo de cizallamiento | -269.0 °C | 80 GPa Show Material materials with Módulo de cizallamiento of 80 GPa |
-200.0 °C | 79.8 GPa Show Material materials with Módulo de cizallamiento of 79.8 GPa | |
-150.0 °C | 79 GPa Show Material materials with Módulo de cizallamiento of 79 GPa | |
-100.0 °C | 78.2 GPa Show Material materials with Módulo de cizallamiento of 78.2 GPa | |
-50.0 °C | 77.1 GPa Show Material materials with Módulo de cizallamiento of 77.1 GPa | |
27.0 °C | 75.4 GPa Show Material materials with Módulo de cizallamiento of 75.4 GPa | |
Módulo elástico | -269.0 °C | 205.5 GPa Show Material materials with Módulo elástico of 205.5 GPa |
-200.0 °C | 205.2 GPa Show Material materials with Módulo elástico of 205.2 GPa | |
-150.0 °C | 203.4 GPa Show Material materials with Módulo elástico of 203.4 GPa | |
-100.0 °C | 201 - 201.4 GPa Show Material materials with Módulo elástico of 201 - 201.4 GPa | |
-50.0 °C | 198.9 GPa Show Material materials with Módulo elástico of 198.9 GPa | |
20.0 °C | 195 GPa Show Material materials with Módulo elástico of 195 GPa | |
27.0 °C | 195.1 GPa Show Material materials with Módulo elástico of 195.1 GPa | |
100.0 °C | 190 GPa Show Material materials with Módulo elástico of 190 GPa | |
200.0 °C | 184 GPa Show Material materials with Módulo elástico of 184 GPa | |
300.0 °C | 178 GPa Show Material materials with Módulo elástico of 178 GPa | |
400.0 °C | 170 GPa Show Material materials with Módulo elástico of 170 GPa | |
Resistencia a la tracción | 20.0 °C | 640 - 840 MPa Show Material materials with Resistencia a la tracción of 640 - 840 MPa |
Aplicaciones térmicas
Property | Temperature | Value |
---|---|---|
Calor específico | -100.0 °C | 442 J/(kg·K) Show Material materials with Calor específico of 442 J/(kg·K) |
20.0 °C | 464 J/(kg·K) Show Material materials with Calor específico of 464 J/(kg·K) | |
100.0 °C | 479 J/(kg·K) Show Material materials with Calor específico of 479 J/(kg·K) | |
200.0 °C | 495 J/(kg·K) Show Material materials with Calor específico of 495 J/(kg·K) | |
300.0 °C | 511 J/(kg·K) Show Material materials with Calor específico of 511 J/(kg·K) | |
400.0 °C | 528 J/(kg·K) Show Material materials with Calor específico of 528 J/(kg·K) | |
Coeficiente de dilatación térmica | -100.0 °C | 1.02E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.02E-5 1/K |
20.0 °C | 1.1E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.1E-5 1/K | |
100.0 °C | 1.14E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.14E-5 1/K | |
200.0 °C | 1.18E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.18E-5 1/K | |
300.0 °C | 1.21E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.21E-5 1/K | |
400.0 °C | 1.25E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.25E-5 1/K | |
Conductividad térmica | -100.0 °C | 23.9 W/(m·K) Show Material materials with Conductividad térmica of 23.9 W/(m·K) |
20.0 °C | 30.2 W/(m·K) Show Material materials with Conductividad térmica of 30.2 W/(m·K) | |
100.0 °C | 32.8 W/(m·K) Show Material materials with Conductividad térmica of 32.8 W/(m·K) | |
200.0 °C | 34.4 W/(m·K) Show Material materials with Conductividad térmica of 34.4 W/(m·K) | |
300.0 °C | 34.7 W/(m·K) Show Material materials with Conductividad térmica of 34.7 W/(m·K) | |
400.0 °C | 34 W/(m·K) Show Material materials with Conductividad térmica of 34 W/(m·K) | |
Difusividad térmica | 20.0 °C | 8.3 mm²/s Show Material materials with Difusividad térmica of 8.3 mm²/s |
100.0 °C | 8.5 mm²/s Show Material materials with Difusividad térmica of 8.5 mm²/s | |
200.0 °C | 8.4 mm²/s Show Material materials with Difusividad térmica of 8.4 mm²/s | |
300.0 °C | 8 mm²/s Show Material materials with Difusividad térmica of 8 mm²/s | |
400.0 °C | 7.3 mm²/s Show Material materials with Difusividad térmica of 7.3 mm²/s | |
Eléctrico
Property | Temperature | Value |
---|---|---|
Resistividad eléctrica | -100.0 °C | 2.51E-7 Ω·m Show Material materials with Resistividad eléctrica of 2.51E-7 Ω·m |
20.0 °C | 3.22E-7 Ω·m Show Material materials with Resistividad eléctrica of 3.22E-7 Ω·m | |
100.0 °C | 3.73E-7 Ω·m Show Material materials with Resistividad eléctrica of 3.73E-7 Ω·m | |
200.0 °C | 4.4E-7 Ω·m Show Material materials with Resistividad eléctrica of 4.4E-7 Ω·m | |
300.0 °C | 5.19E-7 Ω·m Show Material materials with Resistividad eléctrica of 5.19E-7 Ω·m | |
400.0 °C | 6.13E-7 Ω·m Show Material materials with Resistividad eléctrica of 6.13E-7 Ω·m | |
Chemical properties
Property | Value |
---|---|
Azufre | 0.005 - 0.01 % Show Material materials with Azufre of 0.005 - 0.01 % |
Carbono | 0.1 % Show Material materials with Carbono of 0.1 % |
Fósforo | 0.02 % Show Material materials with Fósforo of 0.02 % |
Manganeso | 0.3 - 0.8 % Show Material materials with Manganeso of 0.3 - 0.8 % |
Molibdeno | 0.1 % Show Material materials with Molibdeno of 0.1 % |
Níquel | 8.5 - 10 % Show Material materials with Níquel of 8.5 - 10 % |
Silicona | 0.35 % Show Material materials with Silicona of 0.35 % |
Vanadio | 0.05 % Show Material materials with Vanadio of 0.05 % |