General
Property | Temperature | Value |
---|---|---|
Densidad | 20.0 °C | 7.76 - 8 g/cm³ Show Material materials with Densidad of 7.76 - 8 g/cm³ |
Mecánica
Property | Temperature | Value | Comment |
---|---|---|---|
Coeficiente de Poisson | 23.0 °C | 0.3 [-] Show Material materials with Coeficiente de Poisson of 0.3 [-] | Typical for Austenitic Stainless Steel |
Dureza Brinell | 20.0 °C | 230 [-] Show Material materials with Dureza Brinell of 230 [-] | |
Elongación | 20.0 °C | 35 % Show Material materials with Elongación of 35 % | |
Elongación transversal | 20.0 °C | 30 % Show Material materials with Elongación transversal of 30 % | |
Hardness, Brinell, trans | 20.0 °C | 230 [-] Show Material materials with Hardness, Brinell, trans of 230 [-] | |
Límite elástico Rp 0,2 | 20.0 °C | 230 MPa Show Material materials with Límite elástico Rp 0,2 of 230 MPa | |
100.0 °C | 205 MPa Show Material materials with Límite elástico Rp 0,2 of 205 MPa | ||
150.0 °C | 190 MPa Show Material materials with Límite elástico Rp 0,2 of 190 MPa | ||
200.0 °C | 175 MPa Show Material materials with Límite elástico Rp 0,2 of 175 MPa | ||
250.0 °C | 160 MPa Show Material materials with Límite elástico Rp 0,2 of 160 MPa | ||
300.0 °C | 145 MPa Show Material materials with Límite elástico Rp 0,2 of 145 MPa | ||
350.0 °C | 135 MPa Show Material materials with Límite elástico Rp 0,2 of 135 MPa | ||
400.0 °C | 125 MPa Show Material materials with Límite elástico Rp 0,2 of 125 MPa | ||
450.0 °C | 115 MPa Show Material materials with Límite elástico Rp 0,2 of 115 MPa | ||
500.0 °C | 110 MPa Show Material materials with Límite elástico Rp 0,2 of 110 MPa | ||
550.0 °C | 105 MPa Show Material materials with Límite elástico Rp 0,2 of 105 MPa | ||
Límite elástico Rp 1,0 | 20.0 °C | 260 MPa Show Material materials with Límite elástico Rp 1,0 of 260 MPa | |
100.0 °C | 235 MPa Show Material materials with Límite elástico Rp 1,0 of 235 MPa | ||
150.0 °C | 220 MPa Show Material materials with Límite elástico Rp 1,0 of 220 MPa | ||
200.0 °C | 205 MPa Show Material materials with Límite elástico Rp 1,0 of 205 MPa | ||
250.0 °C | 190 MPa Show Material materials with Límite elástico Rp 1,0 of 190 MPa | ||
300.0 °C | 175 MPa Show Material materials with Límite elástico Rp 1,0 of 175 MPa | ||
350.0 °C | 165 MPa Show Material materials with Límite elástico Rp 1,0 of 165 MPa | ||
400.0 °C | 155 MPa Show Material materials with Límite elástico Rp 1,0 of 155 MPa | ||
450.0 °C | 145 MPa Show Material materials with Límite elástico Rp 1,0 of 145 MPa | ||
500.0 °C | 140 MPa Show Material materials with Límite elástico Rp 1,0 of 140 MPa | ||
550.0 °C | 135 MPa Show Material materials with Límite elástico Rp 1,0 of 135 MPa | ||
Límite elástico transversal Rp 0,2 | 20.0 °C | 230 MPa Show Material materials with Límite elástico transversal Rp 0,2 of 230 MPa | |
Límite elástico transversal Rp 1,0 | 20.0 °C | 260 MPa Show Material materials with Límite elástico transversal Rp 1,0 of 260 MPa | |
Módulo de cizallamiento | 23.0 °C | 77 GPa Show Material materials with Módulo de cizallamiento of 77 GPa | Typical for Austenitic Stainless Steel |
Módulo elástico | -100.0 °C | 206 GPa Show Material materials with Módulo elástico of 206 GPa | |
20.0 °C | 195 - 196 GPa Show Material materials with Módulo elástico of 195 - 196 GPa | ||
100.0 °C | 190 GPa Show Material materials with Módulo elástico of 190 GPa | ||
200.0 °C | 182 GPa Show Material materials with Módulo elástico of 182 GPa | ||
300.0 °C | 174 GPa Show Material materials with Módulo elástico of 174 GPa | ||
400.0 °C | 166 GPa Show Material materials with Módulo elástico of 166 GPa | ||
500.0 °C | 158 GPa Show Material materials with Módulo elástico of 158 GPa | ||
600.0 °C | 150 GPa Show Material materials with Módulo elástico of 150 GPa | ||
700.0 °C | 142 GPa Show Material materials with Módulo elástico of 142 GPa | ||
800.0 °C | 134 GPa Show Material materials with Módulo elástico of 134 GPa | ||
900.0 °C | 127 GPa Show Material materials with Módulo elástico of 127 GPa | ||
1000.0 °C | 120 GPa Show Material materials with Módulo elástico of 120 GPa | ||
Resistencia a la tracción | 20.0 °C | 530 - 730 MPa Show Material materials with Resistencia a la tracción of 530 - 730 MPa | |
100.0 °C | 500 MPa Show Material materials with Resistencia a la tracción of 500 MPa | ||
150.0 °C | 480 MPa Show Material materials with Resistencia a la tracción of 480 MPa | ||
200.0 °C | 460 MPa Show Material materials with Resistencia a la tracción of 460 MPa | ||
250.0 °C | 450 MPa Show Material materials with Resistencia a la tracción of 450 MPa | ||
300.0 °C | 440 MPa Show Material materials with Resistencia a la tracción of 440 MPa | ||
350.0 °C | 435 MPa Show Material materials with Resistencia a la tracción of 435 MPa | ||
Resistencia a la tracción transversal | 20.0 °C | 530 - 730 MPa Show Material materials with Resistencia a la tracción transversal of 530 - 730 MPa |
Aplicaciones térmicas
Property | Temperature | Value | Comment |
---|---|---|---|
Calor específico | -100.0 °C | 440 J/(kg·K) Show Material materials with Calor específico of 440 J/(kg·K) | |
20.0 °C | 450 - 472 J/(kg·K) Show Material materials with Calor específico of 450 - 472 J/(kg·K) | ||
100.0 °C | 487 J/(kg·K) Show Material materials with Calor específico of 487 J/(kg·K) | ||
200.0 °C | 503 J/(kg·K) Show Material materials with Calor específico of 503 J/(kg·K) | ||
300.0 °C | 512 J/(kg·K) Show Material materials with Calor específico of 512 J/(kg·K) | ||
400.0 °C | 520 J/(kg·K) Show Material materials with Calor específico of 520 J/(kg·K) | ||
500.0 °C | 530 J/(kg·K) Show Material materials with Calor específico of 530 J/(kg·K) | ||
600.0 °C | 541 J/(kg·K) Show Material materials with Calor específico of 541 J/(kg·K) | ||
700.0 °C | 551 J/(kg·K) Show Material materials with Calor específico of 551 J/(kg·K) | ||
800.0 °C | 559 J/(kg·K) Show Material materials with Calor específico of 559 J/(kg·K) | ||
900.0 °C | 565 J/(kg·K) Show Material materials with Calor específico of 565 J/(kg·K) | ||
1000.0 °C | 571 J/(kg·K) Show Material materials with Calor específico of 571 J/(kg·K) | ||
Coeficiente de dilatación térmica | -100.0 °C | 1.49E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.49E-5 1/K | |
20.0 °C | 1.61E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.61E-5 1/K | ||
100.0 °C | 1.58E-5 - 1.67E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.58E-5 - 1.67E-5 1/K | ||
200.0 °C | 1.61E-5 - 1.72E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.61E-5 - 1.72E-5 1/K | ||
300.0 °C | 1.65E-5 - 1.77E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.65E-5 - 1.77E-5 1/K | ||
400.0 °C | 1.69E-5 - 1.81E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.69E-5 - 1.81E-5 1/K | ||
500.0 °C | 1.73E-5 - 1.84E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.73E-5 - 1.84E-5 1/K | ||
600.0 °C | 1.88E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.88E-5 1/K | ||
700.0 °C | 1.91E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.91E-5 1/K | ||
800.0 °C | 1.94E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.94E-5 1/K | ||
900.0 °C | 1.97E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.97E-5 1/K | ||
1000.0 °C | 2E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 2E-5 1/K | ||
Conductividad térmica | 20.0 °C | 11.9 - 12 W/(m·K) Show Material materials with Conductividad térmica of 11.9 - 12 W/(m·K) | |
100.0 °C | 13.3 W/(m·K) Show Material materials with Conductividad térmica of 13.3 W/(m·K) | ||
200.0 °C | 15.1 W/(m·K) Show Material materials with Conductividad térmica of 15.1 W/(m·K) | ||
300.0 °C | 16.7 W/(m·K) Show Material materials with Conductividad térmica of 16.7 W/(m·K) | ||
400.0 °C | 18.3 W/(m·K) Show Material materials with Conductividad térmica of 18.3 W/(m·K) | ||
500.0 °C | 19.8 W/(m·K) Show Material materials with Conductividad térmica of 19.8 W/(m·K) | ||
600.0 °C | 21.3 W/(m·K) Show Material materials with Conductividad térmica of 21.3 W/(m·K) | ||
700.0 °C | 22.8 W/(m·K) Show Material materials with Conductividad térmica of 22.8 W/(m·K) | ||
800.0 °C | 24.3 W/(m·K) Show Material materials with Conductividad térmica of 24.3 W/(m·K) | ||
900.0 °C | 25.7 W/(m·K) Show Material materials with Conductividad térmica of 25.7 W/(m·K) | ||
1000.0 °C | 27.1 W/(m·K) Show Material materials with Conductividad térmica of 27.1 W/(m·K) | ||
Difusividad térmica | 20.0 °C | 3.3 mm²/s Show Material materials with Difusividad térmica of 3.3 mm²/s | |
100.0 °C | 3.4 mm²/s Show Material materials with Difusividad térmica of 3.4 mm²/s | ||
200.0 °C | 3.7 mm²/s Show Material materials with Difusividad térmica of 3.7 mm²/s | ||
300.0 °C | 4.1 mm²/s Show Material materials with Difusividad térmica of 4.1 mm²/s | ||
400.0 °C | 4.3 mm²/s Show Material materials with Difusividad térmica of 4.3 mm²/s | ||
500.0 °C | 4.5 mm²/s Show Material materials with Difusividad térmica of 4.5 mm²/s | ||
600.0 °C | 4.7 mm²/s Show Material materials with Difusividad térmica of 4.7 mm²/s | ||
700.0 °C | 5 mm²/s Show Material materials with Difusividad térmica of 5 mm²/s | ||
800.0 °C | 5.4 mm²/s Show Material materials with Difusividad térmica of 5.4 mm²/s | ||
900.0 °C | 5.7 mm²/s Show Material materials with Difusividad térmica of 5.7 mm²/s | ||
1000.0 °C | 5.8 mm²/s Show Material materials with Difusividad térmica of 5.8 mm²/s | ||
Temperatura de fusión | 1230 - 1480 °C Show Material materials with Temperatura de fusión of 1230 - 1480 °C | Typical for Austenitic Stainless Steel |
Eléctrico
Property | Temperature | Value |
---|---|---|
Resistividad eléctrica | 20.0 °C | 9.59E-7 - 1E-6 Ω·m Show Material materials with Resistividad eléctrica of 9.59E-7 - 1E-6 Ω·m |
100.0 °C | 1.01E-6 Ω·m Show Material materials with Resistividad eléctrica of 1.01E-6 Ω·m | |
200.0 °C | 1.05E-6 Ω·m Show Material materials with Resistividad eléctrica of 1.05E-6 Ω·m | |
300.0 °C | 1.1E-6 Ω·m Show Material materials with Resistividad eléctrica of 1.1E-6 Ω·m | |
400.0 °C | 1.13E-6 Ω·m Show Material materials with Resistividad eléctrica of 1.13E-6 Ω·m | |
500.0 °C | 1.17E-6 Ω·m Show Material materials with Resistividad eléctrica of 1.17E-6 Ω·m | |
600.0 °C | 1.19E-6 Ω·m Show Material materials with Resistividad eléctrica of 1.19E-6 Ω·m | |
700.0 °C | 1.22E-6 Ω·m Show Material materials with Resistividad eléctrica of 1.22E-6 Ω·m | |
800.0 °C | 1.24E-6 Ω·m Show Material materials with Resistividad eléctrica of 1.24E-6 Ω·m | |
900.0 °C | 1.26E-6 Ω·m Show Material materials with Resistividad eléctrica of 1.26E-6 Ω·m | |
1000.0 °C | 1.28E-6 Ω·m Show Material materials with Resistividad eléctrica of 1.28E-6 Ω·m | |
Chemical properties
Property | Value |
---|---|
Azufre | 0.01 % Show Material materials with Azufre of 0.01 % |
Carbono | 0.02 % Show Material materials with Carbono of 0.02 % |
Cobre | 1.2 - 2 % Show Material materials with Cobre of 1.2 - 2 % |
Cromo | 19 - 21 % Show Material materials with Cromo of 19 - 21 % |
Fósforo | 0.03 % Show Material materials with Fósforo of 0.03 % |
Manganeso | 2 % Show Material materials with Manganeso of 2 % |
Molibdeno | 4 - 5 % Show Material materials with Molibdeno of 4 - 5 % |
Nitrógeno | 0.15 % Show Material materials with Nitrógeno of 0.15 % |
Níquel | 24 - 26 % Show Material materials with Níquel of 24 - 26 % |
Silicona | 0.7 % Show Material materials with Silicona of 0.7 % |