EN 10025-6 Grade S550QL1 quenched and tempered (+QT)

View suppliers (1)
Want to keep this datasheet? Save it now in your required format

Description

S550QL1 is a tempered and weldable fine grained steel. yield point: >550 N/mm² application: welded steel constructions of various types, e.g. bridges and load-carrying constructions as well as transport vehicles, lifting and earthmoving machines. application limits: at -60°C is warranted a notch impact energy of 30 J (longitudinal test specimen) cold formability: for nominal size < 16 mm bending radius in transversal direction 3xs in longitudinal direction 4xs (s= nominal thickness) hot forming property: allowed only for stress relieve annealing temperature (max. 580°C) suitability for welding: Steel is weldable according to the common welding methods (EURONORM-INFORMATION Nr. 2 has to be considered)

Related Standards

Equivalent Materials

Los datos sobre este material han sido proporcionados por WIAM.

A menos que se indique lo contrario, todas las medidas corresponden a condiciones de temperatura ambiente. A menos que se indique lo contrario, se utilizan las unidades del SI.
Las normas armonizadas son similares a uno o varios estándares del proveedor. Es posible que algunas normas armonizadas se ajusten al estándar original, mientras que otras pueden quedar fuera de su alcance.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Propiedades

General

PropertyTemperatureValueConditionRelated StandardsShape

Densidad

20 °C

7.84 g/cm³

Show Material materials with Densidad of 7.84 g/cm³

quenched and tempered (+QT)

EN 10025-6, EN 10137-2

Flat

Mecánica

PropertyTemperatureValueConditionRelated StandardsShapeComment

Coeficiente de Poisson

0.3 [-]

Show Material materials with Coeficiente de Poisson of 0.3 [-]

Typical for Steel

Elongación

13.0 %

Show Material materials with Elongación of 13.0 %

Predicted Value, A200

13.4 %

Show Material materials with Elongación of 13.4 %

Predicted Value, A80

18.4 %

Show Material materials with Elongación of 18.4 %

Predicted Value, A80 Transverse

18.8 %

Show Material materials with Elongación of 18.8 %

Predicted Value, A5

19.9 %

Show Material materials with Elongación of 19.9 %

Predicted Value, A50

20 °C

16 %

Show Material materials with Elongación of 16 %

quenched and tempered (+QT)

EN 10137-2, EN 10025-6, VdTÜV WB 257

Sheet, Flat

20 °C

18 %

Show Material materials with Elongación of 18 %

quenched and tempered (+QT)

EN 10137-2

Sheet, Flat

Transverse

Estricción

40.1 %

Show Material materials with Estricción of 40.1 %

Predicted Value

44.7 %

Show Material materials with Estricción of 44.7 %

Predicted Value, Transverse

Límite elástico

302.8 MPa

Show Material materials with Límite elástico of 302.8 MPa

Predicted Value, RP1

329.7 MPa

Show Material materials with Límite elástico of 329.7 MPa

Predicted Value, RP1 Transverse

493 MPa

Show Material materials with Límite elástico of 493 MPa

Predicted Value, RP02 Transverse

541.7 MPa

Show Material materials with Límite elástico of 541.7 MPa

Predicted Value, RP05

623.6 MPa

Show Material materials with Límite elástico of 623.6 MPa

Predicted Value, RP002

20 °C

490 MPa

Show Material materials with Límite elástico of 490 MPa

quenched and tempered (+QT)

EN 10137-2, EN 10025-6, VdTÜV WB 257

Sheet, Flat

20 °C

530 MPa

Show Material materials with Límite elástico of 530 MPa

quenched and tempered (+QT)

EN 10137-2, EN 10025-6, VdTÜV WB 257

Sheet, Flat

20 °C

550 MPa

Show Material materials with Límite elástico of 550 MPa

quenched and tempered (+QT)

EN 10137-2, EN 10025-6, VdTÜV WB 257

Sheet, Flat

20 °C

550 MPa

Show Material materials with Límite elástico of 550 MPa

quenched and tempered (+QT)

EN 10137-2

Sheet, Flat

Transverse

100 °C

530 MPa

Show Material materials with Límite elástico of 530 MPa

quenched and tempered (+QT)

EN 10137-2

Sheet, Flat

RP02

150 °C

510 MPa

Show Material materials with Límite elástico of 510 MPa

quenched and tempered (+QT)

EN 10137-2

Sheet, Flat

RP02

200 °C

475 MPa

Show Material materials with Límite elástico of 475 MPa

quenched and tempered (+QT)

EN 10137-2

Sheet, Flat

RP02

250 °C

455 MPa

Show Material materials with Límite elástico of 455 MPa

quenched and tempered (+QT)

EN 10137-2

Sheet, Flat

RP02

300 °C

440 MPa

Show Material materials with Límite elástico of 440 MPa

quenched and tempered (+QT)

EN 10137-2

Sheet, Flat

RP02

350 °C

425 MPa

Show Material materials with Límite elástico of 425 MPa

quenched and tempered (+QT)

EN 10137-2

Sheet, Flat

RP02

400 °C

410 MPa

Show Material materials with Límite elástico of 410 MPa

quenched and tempered (+QT)

EN 10137-2

Sheet, Flat

RP02

Módulo de cizallamiento

20 °C

80 GPa

Show Material materials with Módulo de cizallamiento of 80 GPa

quenched and tempered (+QT)

EN 10025-6, EN 10137-2

Flat

Módulo elástico

20 °C

210 GPa

Show Material materials with Módulo elástico of 210 GPa

quenched and tempered (+QT)

EN 10025-6, EN 10137-2

Flat

Resistencia a la tracción

20 °C

590 - 820 MPa

Show Material materials with Resistencia a la tracción of 590 - 820 MPa

quenched and tempered (+QT)

EN 10137-2, EN 10025-6, VdTÜV WB 257

Sheet, Flat

20 °C

590 - 770 MPa

Show Material materials with Resistencia a la tracción of 590 - 770 MPa

quenched and tempered (+QT)

EN 10137-2, EN 10025-6, VdTÜV WB 257

Sheet, Flat

20 °C

640 - 820 MPa

Show Material materials with Resistencia a la tracción of 640 - 820 MPa

quenched and tempered (+QT)

EN 10137-2, EN 10025-6, VdTÜV WB 257

Sheet, Flat

20 °C

640 - 770 MPa

Show Material materials with Resistencia a la tracción of 640 - 770 MPa

quenched and tempered (+QT)

EN 10137-2, EN 10025-6, VdTÜV WB 257

Sheet, Flat

20 °C

640 - 820 MPa

Show Material materials with Resistencia a la tracción of 640 - 820 MPa

quenched and tempered (+QT)

EN 10137-2

Sheet, Flat

Transverse

Resistencia al cizallamiento

589.7 MPa

Show Material materials with Resistencia al cizallamiento of 589.7 MPa

Predicted Value

Aplicaciones térmicas

PropertyTemperatureValueConditionRelated StandardsShape

Calor específico

20 °C

430 J/(kg·K)

Show Material materials with Calor específico of 430 J/(kg·K)

quenched and tempered (+QT)

EN 10025-6, EN 10137-2

Flat

Coeficiente de dilatación térmica

100 °C

1.2e-05 1/K

Show Material materials with Coeficiente de dilatación térmica of 1.2e-05 1/K

quenched and tempered (+QT)

EN 10025-6, EN 10137-2

Flat

Conductividad térmica

20 °C

39 W/(m·K)

Show Material materials with Conductividad térmica of 39 W/(m·K)

quenched and tempered (+QT)

EN 10025-6, EN 10137-2

Flat

Eléctrico

PropertyTemperatureValueConditionRelated StandardsShapeComment

Conductividad eléctrica

5 S/m

Show Material materials with Conductividad eléctrica of 5 S/m

Predicted Value

Resistividad eléctrica

20 °C

2.7e-07 Ω·m

Show Material materials with Resistividad eléctrica of 2.7e-07 Ω·m

quenched and tempered (+QT)

EN 10025-6, EN 10137-2

Flat

Chemical properties

PropertyValueConditionRelated StandardsShape

Aluminio

0.015 %

Show Material materials with Aluminio of 0.015 %

quenched and tempered (+QT)

EN 10137-2

Sheet, Flat

Azufre

0.01 %

Show Material materials with Azufre of 0.01 %

quenched and tempered (+QT)

EN 10137-2, EN 10025-6, VdTÜV WB 257

Sheet, Flat

Boro

0.005 %

Show Material materials with Boro of 0.005 %

quenched and tempered (+QT)

EN 10137-2, EN 10025-6, VdTÜV WB 257

Sheet, Flat

Carbono

0.2 %

Show Material materials with Carbono of 0.2 %

quenched and tempered (+QT)

EN 10137-2, EN 10025-6, VdTÜV WB 257

Sheet, Flat

Circonio

0.12 %

Show Material materials with Circonio of 0.12 %

quenched and tempered (+QT)

EN 10137-2

Sheet, Flat

0.15 %

Show Material materials with Circonio of 0.15 %

quenched and tempered (+QT)

EN 10137-2, EN 10025-6, VdTÜV WB 257

Sheet, Flat

Cobre

0.5 %

Show Material materials with Cobre of 0.5 %

quenched and tempered (+QT)

EN 10137-2, EN 10025-6, VdTÜV WB 257

Sheet, Flat

Cromo

1.5 %

Show Material materials with Cromo of 1.5 %

quenched and tempered (+QT)

EN 10137-2, EN 10025-6, VdTÜV WB 257

Sheet, Flat

Fósforo

0.02 %

Show Material materials with Fósforo of 0.02 %

quenched and tempered (+QT)

EN 10137-2, EN 10025-6, VdTÜV WB 257

Sheet, Flat

Manganeso

1.6 %

Show Material materials with Manganeso of 1.6 %

quenched and tempered (+QT)

EN 10137-2

Sheet, Flat

1.7 %

Show Material materials with Manganeso of 1.7 %

quenched and tempered (+QT)

EN 10137-2, EN 10025-6, VdTÜV WB 257

Sheet, Flat

Molibdeno

0.6 %

Show Material materials with Molibdeno of 0.6 %

quenched and tempered (+QT)

EN 10137-2

Sheet, Flat

0.7 %

Show Material materials with Molibdeno of 0.7 %

quenched and tempered (+QT)

EN 10137-2, EN 10025-6, VdTÜV WB 257

Sheet, Flat

Niobio

0.06 %

Show Material materials with Niobio of 0.06 %

quenched and tempered (+QT)

EN 10137-2, EN 10025-6, VdTÜV WB 257

Sheet, Flat

Nitrógeno

0.015 %

Show Material materials with Nitrógeno of 0.015 %

quenched and tempered (+QT)

EN 10137-2, EN 10025-6, VdTÜV WB 257

Sheet, Flat

Níquel

2 %

Show Material materials with Níquel of 2 %

quenched and tempered (+QT)

EN 10137-2, EN 10025-6, VdTÜV WB 257

Sheet, Flat

Silicona

0.8 %

Show Material materials with Silicona of 0.8 %

quenched and tempered (+QT)

EN 10137-2, EN 10025-6, VdTÜV WB 257

Sheet, Flat

Titanio

0.05 %

Show Material materials with Titanio of 0.05 %

quenched and tempered (+QT)

EN 10137-2, EN 10025-6, VdTÜV WB 257

Sheet, Flat

Vanadio

0.12 %

Show Material materials with Vanadio of 0.12 %

quenched and tempered (+QT)

EN 10137-2, EN 10025-6, VdTÜV WB 257

Sheet, Flat

Technological properties

Property
Supplier Disclaimer