General
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Densidad | 20 °C | 7.84 g/cm³ Show Material materials with Densidad of 7.84 g/cm³ | quenched and tempered (+QT) | EN 10025-6, EN 10113-3 | Flat |
Mecánica
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Coeficiente de Poisson | 0.3 [-] Show Material materials with Coeficiente de Poisson of 0.3 [-] | Typical for Steel | ||||
Elongación | 10.5 % Show Material materials with Elongación of 10.5 % | Predicted Value, A80 | ||||
10.8 % Show Material materials with Elongación of 10.8 % | Predicted Value, A50 | |||||
12.6 % Show Material materials with Elongación of 12.6 % | Predicted Value, A200 | |||||
12.6 % Show Material materials with Elongación of 12.6 % | Predicted Value, Transverse | |||||
17.8 % Show Material materials with Elongación of 17.8 % | Predicted Value, A5 | |||||
18.3 % Show Material materials with Elongación of 18.3 % | Predicted Value, A80 Transverse | |||||
20 °C | 10 % Show Material materials with Elongación of 10 % | quenched and tempered (+QT) | EN 10137-2, EN 10025-6, EN 10113-3 | Sheet, Flat | ||
Límite elástico | 313.5 MPa Show Material materials with Límite elástico of 313.5 MPa | Predicted Value, RP1 | ||||
329.7 MPa Show Material materials with Límite elástico of 329.7 MPa | Predicted Value, RP1 Transverse | |||||
541.7 MPa Show Material materials with Límite elástico of 541.7 MPa | Predicted Value, RP05 | |||||
604.8 MPa Show Material materials with Límite elástico of 604.8 MPa | Predicted Value, RP02 Transverse | |||||
616.3 MPa Show Material materials with Límite elástico of 616.3 MPa | Predicted Value, Transverse | |||||
800.6 MPa Show Material materials with Límite elástico of 800.6 MPa | Predicted Value, RP002 | |||||
858.3 MPa Show Material materials with Límite elástico of 858.3 MPa | Predicted Value, RP02 | |||||
20 °C | 960 MPa Show Material materials with Límite elástico of 960 MPa | quenched and tempered (+QT) | EN 10137-2, EN 10025-6, EN 10113-3 | Sheet, Flat | ||
Módulo elástico | 20 °C | 210 GPa Show Material materials with Módulo elástico of 210 GPa | quenched and tempered (+QT) | EN 10025-6, EN 10113-3 | Flat | |
Resistencia a la tracción | 20 °C | 980 - 1150 MPa Show Material materials with Resistencia a la tracción of 980 - 1150 MPa | quenched and tempered (+QT) | EN 10137-2, EN 10025-6, EN 10113-3 | Sheet, Flat |
Aplicaciones térmicas
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Calor específico | 20 °C | 440 J/(kg·K) Show Material materials with Calor específico of 440 J/(kg·K) | quenched and tempered (+QT) | EN 10025-6, EN 10113-3 | Flat |
Coeficiente de dilatación térmica | 100 °C | 1.2e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 1.2e-05 1/K | quenched and tempered (+QT) | EN 10025-6, EN 10113-3 | Flat |
Conductividad térmica | 20 °C | 38 W/(m·K) Show Material materials with Conductividad térmica of 38 W/(m·K) | quenched and tempered (+QT) | EN 10025-6, EN 10113-3 | Flat |
Eléctrico
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Resistividad eléctrica | 20 °C | 2.8e-07 Ω·m Show Material materials with Resistividad eléctrica of 2.8e-07 Ω·m | quenched and tempered (+QT) | EN 10025-6, EN 10113-3 | Flat |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Azufre | 0.01 % Show Material materials with Azufre of 0.01 % | quenched and tempered (+QT) | EN 10137-2, EN 10025-6, EN 10113-3 | Sheet, Flat |
Boro | 0.005 % Show Material materials with Boro of 0.005 % | quenched and tempered (+QT) | EN 10137-2, EN 10025-6, EN 10113-3 | Sheet, Flat |
Carbono | 0.2 % Show Material materials with Carbono of 0.2 % | quenched and tempered (+QT) | EN 10137-2, EN 10025-6, EN 10113-3 | Sheet, Flat |
Circonio | 0.15 % Show Material materials with Circonio of 0.15 % | quenched and tempered (+QT) | EN 10137-2, EN 10025-6, EN 10113-3 | Sheet, Flat |
Cobre | 0.5 % Show Material materials with Cobre of 0.5 % | quenched and tempered (+QT) | EN 10137-2, EN 10025-6, EN 10113-3 | Sheet, Flat |
Cromo | 1.5 % Show Material materials with Cromo of 1.5 % | quenched and tempered (+QT) | EN 10137-2, EN 10025-6, EN 10113-3 | Sheet, Flat |
Fósforo | 0.02 % Show Material materials with Fósforo of 0.02 % | quenched and tempered (+QT) | EN 10137-2, EN 10025-6, EN 10113-3 | Sheet, Flat |
Manganeso | 1.7 % Show Material materials with Manganeso of 1.7 % | quenched and tempered (+QT) | EN 10137-2, EN 10025-6, EN 10113-3 | Sheet, Flat |
Molibdeno | 0.7 % Show Material materials with Molibdeno of 0.7 % | quenched and tempered (+QT) | EN 10137-2, EN 10025-6, EN 10113-3 | Sheet, Flat |
Niobio | 0.06 % Show Material materials with Niobio of 0.06 % | quenched and tempered (+QT) | EN 10137-2, EN 10025-6, EN 10113-3 | Sheet, Flat |
Nitrógeno | 0.015 % Show Material materials with Nitrógeno of 0.015 % | quenched and tempered (+QT) | EN 10137-2, EN 10025-6, EN 10113-3 | Sheet, Flat |
Níquel | 2 % Show Material materials with Níquel of 2 % | quenched and tempered (+QT) | EN 10137-2, EN 10025-6, EN 10113-3 | Sheet, Flat |
Silicona | 0.8 % Show Material materials with Silicona of 0.8 % | quenched and tempered (+QT) | EN 10137-2, EN 10025-6, EN 10113-3 | Sheet, Flat |
Titanio | 0.05 % Show Material materials with Titanio of 0.05 % | quenched and tempered (+QT) | EN 10137-2, EN 10025-6, EN 10113-3 | Sheet, Flat |
Vanadio | 0.12 % Show Material materials with Vanadio of 0.12 % | quenched and tempered (+QT) | EN 10137-2, EN 10025-6, EN 10113-3 | Sheet, Flat |
Technological properties
Property | ||
---|---|---|
Supplier Disclaimer | The given information is a rough description and some properties can depend on various factors such as product thickness. Please contact the supplier or refer to the related norm or standard for further information. |