General
Property | Temperature | Value |
---|---|---|
Densidad | 20.0 °C | 8 g/cm³ Show Material materials with Densidad of 8 g/cm³ |
27.0 °C | 7.95 g/cm³ Show Material materials with Densidad of 7.95 g/cm³ | |
Mecánica
Property | Temperature | Value |
---|---|---|
Coeficiente de Poisson | -269.0 °C | 0.28 [-] Show Material materials with Coeficiente de Poisson of 0.28 [-] |
-200.0 °C | 0.28 [-] Show Material materials with Coeficiente de Poisson of 0.28 [-] | |
-150.0 °C | 0.28 [-] Show Material materials with Coeficiente de Poisson of 0.28 [-] | |
-100.0 °C | 0.29 [-] Show Material materials with Coeficiente de Poisson of 0.29 [-] | |
-50.0 °C | 0.29 [-] Show Material materials with Coeficiente de Poisson of 0.29 [-] | |
27.0 °C | 0.29 [-] Show Material materials with Coeficiente de Poisson of 0.29 [-] | |
Elongación | 20.0 °C | 15 % Show Material materials with Elongación of 15 % |
Límite elástico Rp 0,2 | 20.0 °C | 600 MPa Show Material materials with Límite elástico Rp 0,2 of 600 MPa |
50.0 °C | 592 MPa Show Material materials with Límite elástico Rp 0,2 of 592 MPa | |
100.0 °C | 580 MPa Show Material materials with Límite elástico Rp 0,2 of 580 MPa | |
150.0 °C | 570 MPa Show Material materials with Límite elástico Rp 0,2 of 570 MPa | |
200.0 °C | 560 MPa Show Material materials with Límite elástico Rp 0,2 of 560 MPa | |
250.0 °C | 550 MPa Show Material materials with Límite elástico Rp 0,2 of 550 MPa | |
300.0 °C | 540 MPa Show Material materials with Límite elástico Rp 0,2 of 540 MPa | |
350.0 °C | 530 MPa Show Material materials with Límite elástico Rp 0,2 of 530 MPa | |
400.0 °C | 520 MPa Show Material materials with Límite elástico Rp 0,2 of 520 MPa | |
450.0 °C | 510 MPa Show Material materials with Límite elástico Rp 0,2 of 510 MPa | |
500.0 °C | 490 MPa Show Material materials with Límite elástico Rp 0,2 of 490 MPa | |
550.0 °C | 460 MPa Show Material materials with Límite elástico Rp 0,2 of 460 MPa | |
600.0 °C | 430 MPa Show Material materials with Límite elástico Rp 0,2 of 430 MPa | |
650.0 °C | 380 MPa Show Material materials with Límite elástico Rp 0,2 of 380 MPa | |
Módulo de cizallamiento | -269.0 °C | 80.9 GPa Show Material materials with Módulo de cizallamiento of 80.9 GPa |
-200.0 °C | 80.6 GPa Show Material materials with Módulo de cizallamiento of 80.6 GPa | |
-150.0 °C | 79.6 GPa Show Material materials with Módulo de cizallamiento of 79.6 GPa | |
-100.0 °C | 78.2 GPa Show Material materials with Módulo de cizallamiento of 78.2 GPa | |
-50.0 °C | 76.7 GPa Show Material materials with Módulo de cizallamiento of 76.7 GPa | |
27.0 °C | 74.4 GPa Show Material materials with Módulo de cizallamiento of 74.4 GPa | |
Módulo elástico | -269.0 °C | 206.7 GPa Show Material materials with Módulo elástico of 206.7 GPa |
-200.0 °C | 206.3 GPa Show Material materials with Módulo elástico of 206.3 GPa | |
-150.0 °C | 204.6 GPa Show Material materials with Módulo elástico of 204.6 GPa | |
-100.0 °C | 200.9 GPa Show Material materials with Módulo elástico of 200.9 GPa | |
-50.0 °C | 197.8 GPa Show Material materials with Módulo elástico of 197.8 GPa | |
20.0 °C | 211 GPa Show Material materials with Módulo elástico of 211 GPa | |
27.0 °C | 192.5 GPa Show Material materials with Módulo elástico of 192.5 GPa | |
100.0 °C | 206 GPa Show Material materials with Módulo elástico of 206 GPa | |
200.0 °C | 200 GPa Show Material materials with Módulo elástico of 200 GPa | |
300.0 °C | 192 GPa Show Material materials with Módulo elástico of 192 GPa | |
400.0 °C | 183 GPa Show Material materials with Módulo elástico of 183 GPa | |
500.0 °C | 173 GPa Show Material materials with Módulo elástico of 173 GPa | |
600.0 °C | 162 GPa Show Material materials with Módulo elástico of 162 GPa | |
Resistencia a la tracción | 20.0 °C | 900 - 1150 MPa Show Material materials with Resistencia a la tracción of 900 - 1150 MPa |
400.0 °C | 720 MPa Show Material materials with Resistencia a la tracción of 720 MPa | |
450.0 °C | 710 MPa Show Material materials with Resistencia a la tracción of 710 MPa | |
500.0 °C | 700 MPa Show Material materials with Resistencia a la tracción of 700 MPa | |
550.0 °C | 690 MPa Show Material materials with Resistencia a la tracción of 690 MPa | |
600.0 °C | 670 MPa Show Material materials with Resistencia a la tracción of 670 MPa | |
Aplicaciones térmicas
Property | Temperature | Value |
---|---|---|
Coeficiente de dilatación térmica | 100.0 °C | 1.7E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.7E-5 1/K |
200.0 °C | 1.75E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.75E-5 1/K | |
300.0 °C | 1.78E-5 - 1.83E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.78E-5 - 1.83E-5 1/K | |
400.0 °C | 1.8E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.8E-5 1/K | |
500.0 °C | 1.82E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.82E-5 1/K | |
600.0 °C | 1.85E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.85E-5 1/K | |
Temperatura máx. de funcionamiento, largo | 0 - 700 °C Show Material materials with Temperatura máx. de funcionamiento, largo of 0 - 700 °C |
Chemical properties
Property | Value |
---|---|
Aluminio | 0.35 % Show Material materials with Aluminio of 0.35 % |
Azufre | 0.015 % Show Material materials with Azufre of 0.015 % |
Boro | 0.003 - 0.01 % Show Material materials with Boro of 0.003 - 0.01 % |
Carbono | 0.03 - 0.08 % Show Material materials with Carbono of 0.03 - 0.08 % |
Cromo | 13.5 - 16 % Show Material materials with Cromo of 13.5 - 16 % |
Fósforo | 0.03 % Show Material materials with Fósforo of 0.03 % |
Manganeso | 1 - 2 % Show Material materials with Manganeso of 1 - 2 % |
Molibdeno | 1 - 1.5 % Show Material materials with Molibdeno of 1 - 1.5 % |
Níquel | 24 - 27 % Show Material materials with Níquel of 24 - 27 % |
Silicona | 1 % Show Material materials with Silicona of 1 % |
Titanio | 1.9 - 2.3 % Show Material materials with Titanio of 1.9 - 2.3 % |
Vanadio | 0.1 - 0.5 % Show Material materials with Vanadio of 0.1 - 0.5 % |