General
Property | Temperature | Value |
---|---|---|
Densidad | 20.0 °C | 7.98 - 8 g/cm³ Show Material materials with Densidad of 7.98 - 8 g/cm³ |
Mecánica
Property | Temperature | Value | Comment |
---|---|---|---|
Coeficiente de Poisson | 23.0 °C | 0.3 [-] Show Material materials with Coeficiente de Poisson of 0.3 [-] | Typical for Austenitic Stainless Steel |
Elongación A80 transversal | 20.0 °C | 35 % Show Material materials with Elongación A80 transversal of 35 % | |
Elongación transversal | 20.0 °C | 40 % Show Material materials with Elongación transversal of 40 % | |
Límite elástico Rp 0,2 | 50.0 °C | 239 MPa Show Material materials with Límite elástico Rp 0,2 of 239 MPa | |
100.0 °C | 205 MPa Show Material materials with Límite elástico Rp 0,2 of 205 MPa | ||
150.0 °C | 187 MPa Show Material materials with Límite elástico Rp 0,2 of 187 MPa | ||
200.0 °C | 170 MPa Show Material materials with Límite elástico Rp 0,2 of 170 MPa | ||
250.0 °C | 159 MPa Show Material materials with Límite elástico Rp 0,2 of 159 MPa | ||
300.0 °C | 148 MPa Show Material materials with Límite elástico Rp 0,2 of 148 MPa | ||
350.0 °C | 141 MPa Show Material materials with Límite elástico Rp 0,2 of 141 MPa | ||
400.0 °C | 134 MPa Show Material materials with Límite elástico Rp 0,2 of 134 MPa | ||
450.0 °C | 130 MPa Show Material materials with Límite elástico Rp 0,2 of 130 MPa | ||
500.0 °C | 127 MPa Show Material materials with Límite elástico Rp 0,2 of 127 MPa | ||
550.0 °C | 124 MPa Show Material materials with Límite elástico Rp 0,2 of 124 MPa | ||
600.0 °C | 121 MPa Show Material materials with Límite elástico Rp 0,2 of 121 MPa | ||
Límite elástico Rp 1,0 | 50.0 °C | 277 MPa Show Material materials with Límite elástico Rp 1,0 of 277 MPa | |
100.0 °C | 240 MPa Show Material materials with Límite elástico Rp 1,0 of 240 MPa | ||
150.0 °C | 220 MPa Show Material materials with Límite elástico Rp 1,0 of 220 MPa | ||
200.0 °C | 200 MPa Show Material materials with Límite elástico Rp 1,0 of 200 MPa | ||
250.0 °C | 189 MPa Show Material materials with Límite elástico Rp 1,0 of 189 MPa | ||
300.0 °C | 178 MPa Show Material materials with Límite elástico Rp 1,0 of 178 MPa | ||
350.0 °C | 171 MPa Show Material materials with Límite elástico Rp 1,0 of 171 MPa | ||
400.0 °C | 164 MPa Show Material materials with Límite elástico Rp 1,0 of 164 MPa | ||
450.0 °C | 160 MPa Show Material materials with Límite elástico Rp 1,0 of 160 MPa | ||
500.0 °C | 157 MPa Show Material materials with Límite elástico Rp 1,0 of 157 MPa | ||
550.0 °C | 154 MPa Show Material materials with Límite elástico Rp 1,0 of 154 MPa | ||
600.0 °C | 151 MPa Show Material materials with Límite elástico Rp 1,0 of 151 MPa | ||
Límite elástico transversal Rp 0,2 | 20.0 °C | 260 - 300 MPa Show Material materials with Límite elástico transversal Rp 0,2 of 260 - 300 MPa | |
Límite elástico transversal Rp 1,0 | 20.0 °C | 300 - 330 MPa Show Material materials with Límite elástico transversal Rp 1,0 of 300 - 330 MPa | |
Módulo de cizallamiento | 23.0 °C | 77 GPa Show Material materials with Módulo de cizallamiento of 77 GPa | Typical for Austenitic Stainless Steel |
Módulo elástico | -100.0 °C | 206 GPa Show Material materials with Módulo elástico of 206 GPa | |
20.0 °C | 196 - 200 GPa Show Material materials with Módulo elástico of 196 - 200 GPa | ||
100.0 °C | 190 GPa Show Material materials with Módulo elástico of 190 GPa | ||
200.0 °C | 182 - 185 GPa Show Material materials with Módulo elástico of 182 - 185 GPa | ||
300.0 °C | 174 - 175 GPa Show Material materials with Módulo elástico of 174 - 175 GPa | ||
400.0 °C | 166 - 170 GPa Show Material materials with Módulo elástico of 166 - 170 GPa | ||
500.0 °C | 158 - 160 GPa Show Material materials with Módulo elástico of 158 - 160 GPa | ||
600.0 °C | 150 - 155 GPa Show Material materials with Módulo elástico of 150 - 155 GPa | ||
700.0 °C | 142 - 145 GPa Show Material materials with Módulo elástico of 142 - 145 GPa | ||
800.0 °C | 134 - 140 GPa Show Material materials with Módulo elástico of 134 - 140 GPa | ||
900.0 °C | 127 - 135 GPa Show Material materials with Módulo elástico of 127 - 135 GPa | ||
1000.0 °C | 120 - 125 GPa Show Material materials with Módulo elástico of 120 - 125 GPa | ||
Resistencia a la tracción | 20.0 °C | 550 - 780 MPa Show Material materials with Resistencia a la tracción of 550 - 780 MPa | |
50.0 °C | 529 MPa Show Material materials with Resistencia a la tracción of 529 MPa | ||
100.0 °C | 495 MPa Show Material materials with Resistencia a la tracción of 495 MPa | ||
150.0 °C | 472 MPa Show Material materials with Resistencia a la tracción of 472 MPa | ||
200.0 °C | 450 MPa Show Material materials with Resistencia a la tracción of 450 MPa | ||
250.0 °C | 440 MPa Show Material materials with Resistencia a la tracción of 440 MPa | ||
300.0 °C | 430 MPa Show Material materials with Resistencia a la tracción of 430 MPa | ||
350.0 °C | 425 MPa Show Material materials with Resistencia a la tracción of 425 MPa | ||
400.0 °C | 420 MPa Show Material materials with Resistencia a la tracción of 420 MPa | ||
450.0 °C | 410 MPa Show Material materials with Resistencia a la tracción of 410 MPa | ||
500.0 °C | 400 MPa Show Material materials with Resistencia a la tracción of 400 MPa | ||
550.0 °C | 385 MPa Show Material materials with Resistencia a la tracción of 385 MPa | ||
600.0 °C | 365 MPa Show Material materials with Resistencia a la tracción of 365 MPa | ||
Resistencia a la tracción transversal | 20.0 °C | 550 - 780 MPa Show Material materials with Resistencia a la tracción transversal of 550 - 780 MPa |
Aplicaciones térmicas
Property | Temperature | Value | Comment |
---|---|---|---|
Calor específico | -100.0 °C | 440 J/(kg·K) Show Material materials with Calor específico of 440 J/(kg·K) | |
20.0 °C | 450 - 472 J/(kg·K) Show Material materials with Calor específico of 450 - 472 J/(kg·K) | ||
100.0 °C | 487 J/(kg·K) Show Material materials with Calor específico of 487 J/(kg·K) | ||
200.0 °C | 503 J/(kg·K) Show Material materials with Calor específico of 503 J/(kg·K) | ||
300.0 °C | 512 J/(kg·K) Show Material materials with Calor específico of 512 J/(kg·K) | ||
400.0 °C | 520 J/(kg·K) Show Material materials with Calor específico of 520 J/(kg·K) | ||
500.0 °C | 530 J/(kg·K) Show Material materials with Calor específico of 530 J/(kg·K) | ||
600.0 °C | 541 J/(kg·K) Show Material materials with Calor específico of 541 J/(kg·K) | ||
700.0 °C | 551 J/(kg·K) Show Material materials with Calor específico of 551 J/(kg·K) | ||
800.0 °C | 559 J/(kg·K) Show Material materials with Calor específico of 559 J/(kg·K) | ||
900.0 °C | 565 J/(kg·K) Show Material materials with Calor específico of 565 J/(kg·K) | ||
1000.0 °C | 571 J/(kg·K) Show Material materials with Calor específico of 571 J/(kg·K) | ||
Coeficiente de dilatación térmica | -100.0 °C | 1.49E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.49E-5 1/K | |
20.0 °C | 1.61E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.61E-5 1/K | ||
100.0 °C | 1.63E-5 - 1.67E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.63E-5 - 1.67E-5 1/K | ||
200.0 °C | 1.69E-5 - 1.72E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.69E-5 - 1.72E-5 1/K | ||
300.0 °C | 1.73E-5 - 1.77E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.73E-5 - 1.77E-5 1/K | ||
400.0 °C | 1.78E-5 - 1.81E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.78E-5 - 1.81E-5 1/K | ||
500.0 °C | 1.82E-5 - 1.84E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.82E-5 - 1.84E-5 1/K | ||
600.0 °C | 1.85E-5 - 1.88E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.85E-5 - 1.88E-5 1/K | ||
700.0 °C | 1.87E-5 - 1.91E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.87E-5 - 1.91E-5 1/K | ||
800.0 °C | 1.94E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.94E-5 1/K | ||
900.0 °C | 1.97E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.97E-5 1/K | ||
1000.0 °C | 2E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 2E-5 1/K | ||
Conductividad térmica | 20.0 °C | 13.5 - 16 W/(m·K) Show Material materials with Conductividad térmica of 13.5 - 16 W/(m·K) | |
100.0 °C | 15 W/(m·K) Show Material materials with Conductividad térmica of 15 W/(m·K) | ||
200.0 °C | 16.7 W/(m·K) Show Material materials with Conductividad térmica of 16.7 W/(m·K) | ||
300.0 °C | 18.3 W/(m·K) Show Material materials with Conductividad térmica of 18.3 W/(m·K) | ||
400.0 °C | 19.8 W/(m·K) Show Material materials with Conductividad térmica of 19.8 W/(m·K) | ||
500.0 °C | 21.2 W/(m·K) Show Material materials with Conductividad térmica of 21.2 W/(m·K) | ||
600.0 °C | 22.7 W/(m·K) Show Material materials with Conductividad térmica of 22.7 W/(m·K) | ||
700.0 °C | 24.1 W/(m·K) Show Material materials with Conductividad térmica of 24.1 W/(m·K) | ||
800.0 °C | 25.5 W/(m·K) Show Material materials with Conductividad térmica of 25.5 W/(m·K) | ||
900.0 °C | 26.9 W/(m·K) Show Material materials with Conductividad térmica of 26.9 W/(m·K) | ||
1000.0 °C | 28.3 W/(m·K) Show Material materials with Conductividad térmica of 28.3 W/(m·K) | ||
Difusividad térmica | 20.0 °C | 3.6 mm²/s Show Material materials with Difusividad térmica of 3.6 mm²/s | |
100.0 °C | 3.8 mm²/s Show Material materials with Difusividad térmica of 3.8 mm²/s | ||
200.0 °C | 4 mm²/s Show Material materials with Difusividad térmica of 4 mm²/s | ||
300.0 °C | 4.4 mm²/s Show Material materials with Difusividad térmica of 4.4 mm²/s | ||
400.0 °C | 4.6 mm²/s Show Material materials with Difusividad térmica of 4.6 mm²/s | ||
500.0 °C | 4.7 mm²/s Show Material materials with Difusividad térmica of 4.7 mm²/s | ||
600.0 °C | 4.9 mm²/s Show Material materials with Difusividad térmica of 4.9 mm²/s | ||
700.0 °C | 5.2 mm²/s Show Material materials with Difusividad térmica of 5.2 mm²/s | ||
800.0 °C | 5.5 mm²/s Show Material materials with Difusividad térmica of 5.5 mm²/s | ||
900.0 °C | 5.8 mm²/s Show Material materials with Difusividad térmica of 5.8 mm²/s | ||
1000.0 °C | 5.9 mm²/s Show Material materials with Difusividad térmica of 5.9 mm²/s | ||
Temperatura de fusión | 1230 - 1480 °C Show Material materials with Temperatura de fusión of 1230 - 1480 °C | Typical for Austenitic Stainless Steel | |
Temperatura máx. de funcionamiento, largo | 600 - 800 °C Show Material materials with Temperatura máx. de funcionamiento, largo of 600 - 800 °C |
Eléctrico
Property | Temperature | Value |
---|---|---|
Resistividad eléctrica | 20.0 °C | 7.7E-7 Ω·m Show Material materials with Resistividad eléctrica of 7.7E-7 Ω·m |
100.0 °C | 8.34E-7 Ω·m Show Material materials with Resistividad eléctrica of 8.34E-7 Ω·m | |
200.0 °C | 9.03E-7 Ω·m Show Material materials with Resistividad eléctrica of 9.03E-7 Ω·m | |
300.0 °C | 9.64E-7 Ω·m Show Material materials with Resistividad eléctrica of 9.64E-7 Ω·m | |
400.0 °C | 1.02E-6 Ω·m Show Material materials with Resistividad eléctrica of 1.02E-6 Ω·m | |
500.0 °C | 1.06E-6 Ω·m Show Material materials with Resistividad eléctrica of 1.06E-6 Ω·m | |
600.0 °C | 1.1E-6 Ω·m Show Material materials with Resistividad eléctrica of 1.1E-6 Ω·m | |
700.0 °C | 1.13E-6 Ω·m Show Material materials with Resistividad eléctrica of 1.13E-6 Ω·m | |
800.0 °C | 1.17E-6 Ω·m Show Material materials with Resistividad eléctrica of 1.17E-6 Ω·m | |
900.0 °C | 1.19E-6 Ω·m Show Material materials with Resistividad eléctrica of 1.19E-6 Ω·m | |
1000.0 °C | 1.22E-6 Ω·m Show Material materials with Resistividad eléctrica of 1.22E-6 Ω·m | |
Chemical properties
Property | Value |
---|---|
Azufre | 0.015 % Show Material materials with Azufre of 0.015 % |
Boro | 1.5E-3 - 5E-3 % Show Material materials with Boro of 1.5E-3 - 5E-3 % |
Carbono | 0.04 % Show Material materials with Carbono of 0.04 % |
Cromo | 16 - 18 % Show Material materials with Cromo of 16 - 18 % |
Fósforo | 0.04 % Show Material materials with Fósforo of 0.04 % |
Manganeso | 2 % Show Material materials with Manganeso of 2 % |
Molibdeno | 2 - 3 % Show Material materials with Molibdeno of 2 - 3 % |
Nitrógeno | 0.1 - 0.18 % Show Material materials with Nitrógeno of 0.1 - 0.18 % |
Níquel | 12 - 14 % Show Material materials with Níquel of 12 - 14 % |
Silicona | 0.75 % Show Material materials with Silicona of 0.75 % |