EN 1563 Grade GJS-800-2 heat treatment by manufacturer or by agreement

Want to keep this datasheet? Save it now in your required format

Description

EN-GJS-800-2 (before GGG-80 acc. to DIN 1693/01-73), a pearlitic cast iron with nodular graphite for cast parts of high strength and hardness, e.g. cutter heads, pinions, cast parts of high abrasion load, e.g. rabbles, worm wheel segments for construction machines. This cast iron mark applies to specimen made by machining of separately cast samples. The material is comparable to UNS F 36200 from the USA. The fracture toughness of this make accounts for 14 MPa*m^1/2 (information value). The fatigue strength (Woehler- rotating bending test) accounts for the unnotched specimen (diameter: 10,6 mm) 304 N/mm², for the notched sample 182 N/mm² (unnotched specimen: For annealed ferritic cast iron with nodular graphite (GGG) the fatigue strength approximates the tensile strength x0,5 (Rm) of GGG with a Rm of 370 N/mm². The rate decreases according to the increasing Rm so far until fatigue strength for perlitic and tempered GGG approximates Rm x0,4. The rate continues to increase if the Rm exceed 740 N/mm². Notched specimen: For a sample of 10,6 mm diameter at the notch and a circumferential 45°- V-notch at a radius of 0,25 mm the fatigue strength of annealed GGG increases to a value of the fatigue strength x approx.0,63 of unnotched samples of GGG with a Rm of 370 N/mm². This value decreases according to the rising Rm of ferritic GGG. For GGG of intermediate strength values and for perlitic GGG and for tempered GGG the fatigue strength of notched samples approximates fatigue strength x0,6 of unnotched samples). Pearlite resp. heat-treated martensite are the predominant structure.

Related Standards

Equivalent Materials

Los datos sobre este material han sido proporcionados por WIAM.

A menos que se indique lo contrario, todas las medidas corresponden a condiciones de temperatura ambiente. A menos que se indique lo contrario, se utilizan las unidades del SI.
Las normas armonizadas son similares a uno o varios estándares del proveedor. Es posible que algunas normas armonizadas se ajusten al estándar original, mientras que otras pueden quedar fuera de su alcance.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Propiedades

General

PropertyTemperatureValue

Densidad

20.0 °C

7.2 g/cm³

Show Material materials with Densidad of 7.2 g/cm³

Mecánica

PropertyTemperatureValueComment

Coeficiente de Poisson

20.0 °C

0.28 [-]

Show Material materials with Coeficiente de Poisson of 0.28 [-]

Compressive yield strength

20.0 °C

1150 MPa

Show Material materials with Compressive yield strength of 1150 MPa

Elongación

20.0 °C

2 %

Show Material materials with Elongación of 2 %

Límite elástico Rp 0,2

20.0 °C

480 MPa

Show Material materials with Límite elástico Rp 0,2 of 480 MPa

Módulo de cizallamiento

23.0 °C

63 - 66 GPa

Show Material materials with Módulo de cizallamiento of 63 - 66 GPa

Typical for Ductile (Nodular) Cast Iron

Módulo elástico

20.0 °C

176 GPa

Show Material materials with Módulo elástico of 176 GPa

Resistencia a la tracción

20.0 °C

800 MPa

Show Material materials with Resistencia a la tracción of 800 MPa

Resistencia al cizallamiento

20.0 °C

720 MPa

Show Material materials with Resistencia al cizallamiento of 720 MPa

Aplicaciones térmicas

PropertyTemperatureValueComment

Calor específico

500.0 °C

515 J/(kg·K)

Show Material materials with Calor específico of 515 J/(kg·K)

Coeficiente de dilatación térmica

400.0 °C

1.25E-5 1/K

Show Material materials with Coeficiente de dilatación térmica of 1.25E-5 1/K

Conductividad térmica

20.0 °C

32 W/(m·K)

Show Material materials with Conductividad térmica of 32 W/(m·K)

300.0 °C

31.1 W/(m·K)

Show Material materials with Conductividad térmica of 31.1 W/(m·K)

Temperatura de fusión

1150 - 1200 °C

Show Material materials with Temperatura de fusión of 1150 - 1200 °C

Typical for Ductile (Nodular) Cast Iron

Eléctrico

PropertyTemperatureValue

Resistividad eléctrica

20.0 °C

5.4E-7 Ω·m

Show Material materials with Resistividad eléctrica of 5.4E-7 Ω·m

Chemical properties

PropertyValue

Azufre

0.01 %

Show Material materials with Azufre of 0.01 %

Carbono

3.5 - 3.8 %

Show Material materials with Carbono of 3.5 - 3.8 %

Fósforo

0.1 %

Show Material materials with Fósforo of 0.1 %

Magnesio

0.06 - 0.12 %

Show Material materials with Magnesio of 0.06 - 0.12 %

Manganeso

0.4 %

Show Material materials with Manganeso of 0.4 %

Silicona

2 - 3 %

Show Material materials with Silicona of 2 - 3 %