General
Property | Temperature | Value | Condition | Related Standards |
---|---|---|---|---|
Densidad | 20.0 °C | 2.65 g/cm³ Show Material materials with Densidad of 2.65 g/cm³ | T5 | DIN 1725-2, EN 1676, EN 1706 |
Mecánica
Property | Temperature | Value | Condition | Related Standards | Comment |
---|---|---|---|---|---|
Coeficiente de Poisson | 0.33 [-] Show Material materials with Coeficiente de Poisson of 0.33 [-] | Typical for Cast 3xx.x Series Aluminium | |||
Dureza Brinell | 20.0 °C | 75.0 [-] Show Material materials with Dureza Brinell of 75.0 [-] | T5 | DIN 1725-2, EN 1676, EN 1706 | |
20.0 °C | 80.0 [-] Show Material materials with Dureza Brinell of 80.0 [-] | T5 | DIN 1725-2, EN 1676, EN 1706 | ||
20.0 °C | 80.0 - 110.0 [-] Show Material materials with Dureza Brinell of 80.0 - 110.0 [-] | T5 | DIN 1725-2, EN 1676, EN 1706 | ||
20.0 °C | 85.0 - 115.0 [-] Show Material materials with Dureza Brinell of 85.0 - 115.0 [-] | T5 | DIN 1725-2, EN 1676, EN 1706 | ||
Elongación | 20.0 °C | 0.5 % Show Material materials with Elongación of 0.5 % | T5 | DIN 1725-2, EN 1676, EN 1706 | |
20.0 °C | 1.0 - 3.0 % Show Material materials with Elongación of 1.0 - 3.0 % | T5 | DIN 1725-2, EN 1676, EN 1706 | ||
Módulo de cizallamiento | 2.8 GPa Show Material materials with Módulo de cizallamiento of 2.8 GPa | Typical for Cast 3xx.x Series Aluminium | |||
Módulo elástico | 20.0 °C | 74.0 GPa Show Material materials with Módulo elástico of 74.0 GPa | T5 | DIN 1725-2, EN 1676, EN 1706 | |
Resistencia a la tracción | 20.0 °C | 200.0 MPa Show Material materials with Resistencia a la tracción of 200.0 MPa | T5 | DIN 1725-2, EN 1676, EN 1706 | |
20.0 °C | 220.0 MPa Show Material materials with Resistencia a la tracción of 220.0 MPa | T5 | DIN 1725-2, EN 1676, EN 1706 | ||
20.0 °C | 220.0 - 320.0 MPa Show Material materials with Resistencia a la tracción of 220.0 - 320.0 MPa | T5 | DIN 1725-2, EN 1676, EN 1706 | ||
20.0 °C | 240.0 - 320.0 MPa Show Material materials with Resistencia a la tracción of 240.0 - 320.0 MPa | T5 | DIN 1725-2, EN 1676, EN 1706 |
Aplicaciones térmicas
Property | Temperature | Value | Condition | Related Standards | Comment |
---|---|---|---|---|---|
Calor específico | 20.0 °C | 900.0 J/(kg·K) Show Material materials with Calor específico of 900.0 J/(kg·K) | T5 | DIN 1725-2, EN 1676, EN 1706 | |
Coeficiente de dilatación térmica | 200.0 °C | 2.2e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.2e-05 1/K | T5 | DIN 1725-2, EN 1676, EN 1706 | |
Conductividad térmica | 20.0 °C | 120.0 - 160.0 W/(m·K) Show Material materials with Conductividad térmica of 120.0 - 160.0 W/(m·K) | T5 | DIN 1725-2, EN 1676, EN 1706 | |
Temperatura de fusión | 505.0 - 770.0 °C Show Material materials with Temperatura de fusión of 505.0 - 770.0 °C | Typical for Cast 3xx.x Series Aluminium |
Eléctrico
Property | Temperature | Value | Condition | Related Standards |
---|---|---|---|---|
Conductividad eléctrica | 20.0 °C | 16000000.0 - 22000000.0 S/m Show Material materials with Conductividad eléctrica of 16000000.0 - 22000000.0 S/m | T5 | DIN 1725-2, EN 1676, EN 1706 |
Chemical properties
Property | Value | Condition | Related Standards |
---|---|---|---|
Aluminio | 86.5 % Show Material materials with Aluminio of 86.5 % | T5 | DIN 1725-2, EN 1676, EN 1706 |
Cobre | 0.3 Show Material materials with Cobre of 0.3 | T5 | DIN 1725-2, EN 1676, EN 1706 |
Hierro | 0.6 Show Material materials with Hierro of 0.6 | T5 | DIN 1725-2, EN 1676, EN 1706 |
Magnesio | 0.2 - 0.5 % Show Material materials with Magnesio of 0.2 - 0.5 % | T5 | DIN 1725-2, EN 1676, EN 1706 |
Manganeso | 0.1 - 0.4 % Show Material materials with Manganeso of 0.1 - 0.4 % | T5 | DIN 1725-2, EN 1676, EN 1706 |
Níquel | 0.1 Show Material materials with Níquel of 0.1 | T5 | DIN 1725-2, EN 1676, EN 1706 |
Silicona | 9.0 - 11.0 % Show Material materials with Silicona of 9.0 - 11.0 % | T5 | DIN 1725-2, EN 1676, EN 1706 |
Titanio | 0.15 Show Material materials with Titanio of 0.15 | T5 | DIN 1725-2, EN 1676, EN 1706 |
Zinc | 0.3 Show Material materials with Zinc of 0.3 | T5 | DIN 1725-2, EN 1676, EN 1706 |
Technological properties
Property | ||
---|---|---|
Processing methods | permanent mould casting, sample taken from casting or cast on |