General
Property | Temperature | Value | Comment |
---|---|---|---|
Densidad | 23.0 °C | 7.8 - 7.9 g/cm³ Show Material materials with Densidad of 7.8 - 7.9 g/cm³ | Typical for Low Carbon Steel |
Mecánica
Property | Temperature | Value | Comment |
---|---|---|---|
Coeficiente de Poisson | 23.0 °C | 0.29 [-] Show Material materials with Coeficiente de Poisson of 0.29 [-] | Typical for Low Carbon Steel |
Elongación A50 | 23.0 °C | 21 % Show Material materials with Elongación A50 of 21 % | |
Elongation A200 | 23.0 °C | 18 % Show Material materials with Elongation A200 of 18 % | |
Límite elástico | 23.0 °C | 290 - 345 MPa Show Material materials with Límite elástico of 290 - 345 MPa | |
Módulo de cizallamiento | 23.0 °C | 82 GPa Show Material materials with Módulo de cizallamiento of 82 GPa | Typical for Low Carbon Steel |
Módulo elástico | 23.0 °C | 200 - 215 GPa Show Material materials with Módulo elástico of 200 - 215 GPa | Typical for Low Carbon Steel |
Resistencia a la tracción | 23.0 °C | 435 - 485 MPa Show Material materials with Resistencia a la tracción of 435 - 485 MPa |
Aplicaciones térmicas
Property | Temperature | Value | Comment |
---|---|---|---|
Calor específico | 23.0 °C | 465 J/(kg·K) Show Material materials with Calor específico of 465 J/(kg·K) | Typical for Low Carbon Steel |
Coeficiente de dilatación térmica | 23.0 °C | 1.32E-5 - 1.38E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.32E-5 - 1.38E-5 1/K | Typical for Low Carbon Steel |
Conductividad térmica | 23.0 °C | 25 - 93 W/(m·K) Show Material materials with Conductividad térmica of 25 - 93 W/(m·K) | Typical for Low Carbon Steel |
Temperatura de fusión | 1480 - 1526 °C Show Material materials with Temperatura de fusión of 1480 - 1526 °C | Typical for Low Carbon Steel | |
Temperatura máx. de funcionamiento | 500 °C Show Material materials with Temperatura máx. de funcionamiento of 500 °C | Typical for Carbon Steel |
Eléctrico
Property | Temperature | Value | Comment |
---|---|---|---|
Resistividad eléctrica | 23.0 °C | 1.43E-7 - 1.74E-7 Ω·m Show Material materials with Resistividad eléctrica of 1.43E-7 - 1.74E-7 Ω·m | Typical for Carbon Steel |
Magnético
Property | Value | Comment |
---|---|---|
Temperatura de Curie | 770 °C Show Material materials with Temperatura de Curie of 770 °C | Typical for Low Carbon Steel |
Chemical properties
Property | Value |
---|---|
Azufre | 0.03 % Show Material materials with Azufre of 0.03 % |
Carbono | 0.19 % Show Material materials with Carbono of 0.19 % |
Cobre | 0.25 - 0.4 % Show Material materials with Cobre of 0.25 - 0.4 % |
Cromo | 0.4 - 0.65 % Show Material materials with Cromo of 0.4 - 0.65 % |
Fósforo | 0.03 % Show Material materials with Fósforo of 0.03 % |
Manganeso | 0.8 - 1.25 % Show Material materials with Manganeso of 0.8 - 1.25 % |
Níquel | 0.4 % Show Material materials with Níquel of 0.4 % |
Silicona | 0.3 - 0.65 % Show Material materials with Silicona of 0.3 - 0.65 % |
Vanadio | 0.02 - 0.1 % Show Material materials with Vanadio of 0.02 - 0.1 % |