General
Property | Value | Comment |
---|---|---|
Densidad | 7.8 g/cm³ Show Material materials with Densidad of 7.8 g/cm³ | Typical for Steel |
Mecánica
Property | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|
Coeficiente de Poisson | 0.3 [-] Show Material materials with Coeficiente de Poisson of 0.3 [-] | Typical for Steel | |||
Elongación | 12.6 % Show Material materials with Elongación of 12.6 % | Predicted Value, A200 | |||
14 % Show Material materials with Elongación of 14 % | Quenched and Tempered | ASTM A543 | Plate | A50 | |
16.9 % Show Material materials with Elongación of 16.9 % | Predicted Value, A80 | ||||
18.4 % Show Material materials with Elongación of 18.4 % | Predicted Value, Transverse | ||||
20.2 % Show Material materials with Elongación of 20.2 % | Predicted Value, A80 Transverse | ||||
20.5 % Show Material materials with Elongación of 20.5 % | Predicted Value | ||||
Estricción | 43.5 % Show Material materials with Estricción of 43.5 % | Predicted Value, Transverse | |||
44.8 % Show Material materials with Estricción of 44.8 % | Predicted Value | ||||
Límite elástico | 315.9 MPa Show Material materials with Límite elástico of 315.9 MPa | Predicted Value, RP1 | |||
330.7 MPa Show Material materials with Límite elástico of 330.7 MPa | Predicted Value, RP1 Transverse | ||||
332.5 MPa Show Material materials with Límite elástico of 332.5 MPa | Predicted Value, RP05 | ||||
490 MPa Show Material materials with Límite elástico of 490 MPa | Predicted Value, RP02 Transverse | ||||
494.6 MPa Show Material materials with Límite elástico of 494.6 MPa | Predicted Value, Transverse | ||||
585 MPa Show Material materials with Límite elástico of 585 MPa | Quenched and Tempered | ASTM A543 | Plate | ||
594.3 MPa Show Material materials with Límite elástico of 594.3 MPa | Predicted Value, RP02 | ||||
666.4 MPa Show Material materials with Límite elástico of 666.4 MPa | Predicted Value, RP002 | ||||
Módulo de cizallamiento | 79.4 GPa Show Material materials with Módulo de cizallamiento of 79.4 GPa | Predicted Value | |||
Módulo elástico | 190 - 210 GPa Show Material materials with Módulo elástico of 190 - 210 GPa | Typical for Steel | |||
Resistencia a la tracción | 725 - 860 MPa Show Material materials with Resistencia a la tracción of 725 - 860 MPa | Quenched and Tempered | ASTM A543 | Plate | |
Resistencia al cizallamiento | 618.5 MPa Show Material materials with Resistencia al cizallamiento of 618.5 MPa | Predicted Value |
Aplicaciones térmicas
Property | Value | Comment |
---|---|---|
Calor específico | 458.4 J/(kg·K) Show Material materials with Calor específico of 458.4 J/(kg·K) | Predicted Value |
Coeficiente de dilatación térmica | 11.88 1/K Show Material materials with Coeficiente de dilatación térmica of 11.88 1/K | Predicted Value |
Conductividad térmica | 31.3 W/(m·K) Show Material materials with Conductividad térmica of 31.3 W/(m·K) | Predicted Value |
Eléctrico
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Azufre | 0.02 % Show Material materials with Azufre of 0.02 % | Quenched and Tempered | ASTM A543 | Plate |
Carbono | 0.18 % Show Material materials with Carbono of 0.18 % | Quenched and Tempered | ASTM A543 | Plate |
Cromo | 1 - 1.9 % Show Material materials with Cromo of 1 - 1.9 % | Quenched and Tempered | ASTM A543 | Plate |
Fósforo | 0.02 % Show Material materials with Fósforo of 0.02 % | Quenched and Tempered | ASTM A543 | Plate |
Manganeso | 0.4 % Show Material materials with Manganeso of 0.4 % | Quenched and Tempered | ASTM A543 | Plate |
Molibdeno | 0.2 - 0.65 % Show Material materials with Molibdeno of 0.2 - 0.65 % | Quenched and Tempered | ASTM A543 | Plate |
Níquel | 2 - 3.5 % Show Material materials with Níquel of 2 - 3.5 % | Quenched and Tempered | ASTM A543 | Plate |
Silicona | 0.15 - 0.4 % Show Material materials with Silicona of 0.15 - 0.4 % | Quenched and Tempered | ASTM A543 | Plate |
Technological properties
Property | ||
---|---|---|
Supplier Disclaimer | The given information is a rough description and some properties can depend on various factors such as product thickness. Please contact the supplier or refer to the related norm or standard for further information. |