General
Property | Temperature | Value |
---|---|---|
Densidad | 20.0 °C | 8.9 g/cm³ Show Material materials with Densidad of 8.9 g/cm³ |
Mecánica
Property | Temperature | Value |
---|---|---|
Dureza Vickers | 20.0 °C | 140 [-] Show Material materials with Dureza Vickers of 140 [-] |
Elongación | 20.0 °C | 14 % Show Material materials with Elongación of 14 % |
Elongación transversal | 20.0 °C | 14 % Show Material materials with Elongación transversal of 14 % |
Límite elástico Rp 0,2 | 20.0 °C | 300 MPa Show Material materials with Límite elástico Rp 0,2 of 300 MPa |
50.0 °C | 300 MPa Show Material materials with Límite elástico Rp 0,2 of 300 MPa | |
100.0 °C | 275 MPa Show Material materials with Límite elástico Rp 0,2 of 275 MPa | |
150.0 °C | 265 MPa Show Material materials with Límite elástico Rp 0,2 of 265 MPa | |
200.0 °C | 260 MPa Show Material materials with Límite elástico Rp 0,2 of 260 MPa | |
250.0 °C | 255 MPa Show Material materials with Límite elástico Rp 0,2 of 255 MPa | |
300.0 °C | 245 MPa Show Material materials with Límite elástico Rp 0,2 of 245 MPa | |
350.0 °C | 240 MPa Show Material materials with Límite elástico Rp 0,2 of 240 MPa | |
Límite elástico transversal Rp 0,2 | 20.0 °C | 300 MPa Show Material materials with Límite elástico transversal Rp 0,2 of 300 MPa |
50.0 °C | 300 MPa Show Material materials with Límite elástico transversal Rp 0,2 of 300 MPa | |
100.0 °C | 275 MPa Show Material materials with Límite elástico transversal Rp 0,2 of 275 MPa | |
150.0 °C | 255 - 265 MPa Show Material materials with Límite elástico transversal Rp 0,2 of 255 - 265 MPa | |
200.0 °C | 240 - 260 MPa Show Material materials with Límite elástico transversal Rp 0,2 of 240 - 260 MPa | |
250.0 °C | 255 MPa Show Material materials with Límite elástico transversal Rp 0,2 of 255 MPa | |
300.0 °C | 245 MPa Show Material materials with Límite elástico transversal Rp 0,2 of 245 MPa | |
350.0 °C | 240 MPa Show Material materials with Límite elástico transversal Rp 0,2 of 240 MPa | |
Módulo elástico | -253.0 °C | 161 GPa Show Material materials with Módulo elástico of 161 GPa |
-195.0 °C | 158 GPa Show Material materials with Módulo elástico of 158 GPa | |
-100.0 °C | 155 GPa Show Material materials with Módulo elástico of 155 GPa | |
20.0 °C | 150 GPa Show Material materials with Módulo elástico of 150 GPa | |
50.0 °C | 150 GPa Show Material materials with Módulo elástico of 150 GPa | |
100.0 °C | 149 GPa Show Material materials with Módulo elástico of 149 GPa | |
150.0 °C | 148 GPa Show Material materials with Módulo elástico of 148 GPa | |
200.0 °C | 146 GPa Show Material materials with Módulo elástico of 146 GPa | |
250.0 °C | 144 GPa Show Material materials with Módulo elástico of 144 GPa | |
300.0 °C | 142 GPa Show Material materials with Módulo elástico of 142 GPa | |
350.0 °C | 141 GPa Show Material materials with Módulo elástico of 141 GPa | |
Resistencia a la tracción | 20.0 °C | 410 MPa Show Material materials with Resistencia a la tracción of 410 MPa |
Resistencia a la tracción transversal | 20.0 °C | 410 MPa Show Material materials with Resistencia a la tracción transversal of 410 MPa |
Aplicaciones térmicas
Property | Temperature | Value | Comment |
---|---|---|---|
Calor específico | 23.0 °C | 375 - 398 J/(kg·K) Show Material materials with Calor específico of 375 - 398 J/(kg·K) | Typical for Wrought Copper Nickel Grade |
Coeficiente de dilatación térmica | 300.0 °C | 1.6E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.6E-5 1/K | |
Conductividad térmica | 20.0 °C | 29 W/(m·K) Show Material materials with Conductividad térmica of 29 W/(m·K) | |
Temperatura de fusión | 915 - 1240 °C Show Material materials with Temperatura de fusión of 915 - 1240 °C | Typical for Wrought Copper Nickel Grade |
Chemical properties
Property | Value |
---|---|
Azufre | 0.05 % Show Material materials with Azufre of 0.05 % |
Carbono | 0.05 % Show Material materials with Carbono of 0.05 % |
Cobalto | 0.1 % Show Material materials with Cobalto of 0.1 % |
Estaño | 0.05 % Show Material materials with Estaño of 0.05 % |
Fósforo | 0.02 % Show Material materials with Fósforo of 0.02 % |
Hierro | 0.4 - 1 % Show Material materials with Hierro of 0.4 - 1 % |
Manganeso | 0.5 - 1.5 % Show Material materials with Manganeso of 0.5 - 1.5 % |
Níquel | 30 - 32 % Show Material materials with Níquel of 30 - 32 % |
Plomo | 0.02 % Show Material materials with Plomo of 0.02 % |
Zinc | 0.5 % Show Material materials with Zinc of 0.5 % |