General
Property | Temperature | Value |
---|---|---|
Densidad | 20.0 °C | 8.9 g/cm³ Show Material materials with Densidad of 8.9 g/cm³ |
Mecánica
Property | Temperature | Value |
---|---|---|
Dureza Vickers | 20.0 °C | 120 [-] Show Material materials with Dureza Vickers of 120 [-] |
Elongación | 20.0 °C | 10 - 14 % Show Material materials with Elongación of 10 - 14 % |
Elongación transversal | 20.0 °C | 14 % Show Material materials with Elongación transversal of 14 % |
Elongation A10 | 20.0 °C | 8 % Show Material materials with Elongation A10 of 8 % |
Elongation A100 | 20.0 °C | 6 % Show Material materials with Elongation A100 of 6 % |
Elongation A11.3 | 20.0 °C | 8 % Show Material materials with Elongation A11.3 of 8 % |
Límite elástico Rp 0,2 | 20.0 °C | 150 - 250 MPa Show Material materials with Límite elástico Rp 0,2 of 150 - 250 MPa |
50.0 °C | 250 MPa Show Material materials with Límite elástico Rp 0,2 of 250 MPa | |
100.0 °C | 235 MPa Show Material materials with Límite elástico Rp 0,2 of 235 MPa | |
150.0 °C | 225 MPa Show Material materials with Límite elástico Rp 0,2 of 225 MPa | |
200.0 °C | 220 MPa Show Material materials with Límite elástico Rp 0,2 of 220 MPa | |
250.0 °C | 210 MPa Show Material materials with Límite elástico Rp 0,2 of 210 MPa | |
300.0 °C | 205 MPa Show Material materials with Límite elástico Rp 0,2 of 205 MPa | |
Límite elástico transversal Rp 0,2 | 20.0 °C | 250 MPa Show Material materials with Límite elástico transversal Rp 0,2 of 250 MPa |
50.0 °C | 250 MPa Show Material materials with Límite elástico transversal Rp 0,2 of 250 MPa | |
100.0 °C | 235 MPa Show Material materials with Límite elástico transversal Rp 0,2 of 235 MPa | |
150.0 °C | 210 - 225 MPa Show Material materials with Límite elástico transversal Rp 0,2 of 210 - 225 MPa | |
200.0 °C | 205 - 220 MPa Show Material materials with Límite elástico transversal Rp 0,2 of 205 - 220 MPa | |
250.0 °C | 210 MPa Show Material materials with Límite elástico transversal Rp 0,2 of 210 MPa | |
300.0 °C | 205 MPa Show Material materials with Límite elástico transversal Rp 0,2 of 205 MPa | |
Módulo elástico | -253.0 °C | 153 GPa Show Material materials with Módulo elástico of 153 GPa |
-195.0 °C | 148 GPa Show Material materials with Módulo elástico of 148 GPa | |
-100.0 °C | 142 GPa Show Material materials with Módulo elástico of 142 GPa | |
20.0 °C | 130 GPa Show Material materials with Módulo elástico of 130 GPa | |
50.0 °C | 129 GPa Show Material materials with Módulo elástico of 129 GPa | |
100.0 °C | 128 GPa Show Material materials with Módulo elástico of 128 GPa | |
150.0 °C | 127 GPa Show Material materials with Módulo elástico of 127 GPa | |
200.0 °C | 125 GPa Show Material materials with Módulo elástico of 125 GPa | |
250.0 °C | 122 GPa Show Material materials with Módulo elástico of 122 GPa | |
300.0 °C | 121 GPa Show Material materials with Módulo elástico of 121 GPa | |
Resistencia a la tracción | 20.0 °C | 350 MPa Show Material materials with Resistencia a la tracción of 350 MPa |
Resistencia a la tracción transversal | 20.0 °C | 350 MPa Show Material materials with Resistencia a la tracción transversal of 350 MPa |
Aplicaciones térmicas
Property | Temperature | Value | Comment |
---|---|---|---|
Calor específico | 20.0 °C | 380 J/(kg·K) Show Material materials with Calor específico of 380 J/(kg·K) | |
Coeficiente de dilatación térmica | 23.0 °C | 1.4E-5 - 1.8E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.4E-5 - 1.8E-5 1/K | Typical for Wrought Copper Nickel Grade |
Conductividad térmica | 20.0 °C | 50.2 W/(m·K) Show Material materials with Conductividad térmica of 50.2 W/(m·K) | |
Temperatura de fusión | 915 - 1240 °C Show Material materials with Temperatura de fusión of 915 - 1240 °C | Typical for Wrought Copper Nickel Grade |
Chemical properties
Property | Value |
---|---|
Azufre | 0.05 % Show Material materials with Azufre of 0.05 % |
Carbono | 0.05 % Show Material materials with Carbono of 0.05 % |
Cobalto | 0.1 % Show Material materials with Cobalto of 0.1 % |
Estaño | 0.03 % Show Material materials with Estaño of 0.03 % |
Fósforo | 0.02 % Show Material materials with Fósforo of 0.02 % |
Hierro | 1 - 2 % Show Material materials with Hierro of 1 - 2 % |
Manganeso | 0.5 - 1 % Show Material materials with Manganeso of 0.5 - 1 % |
Níquel | 9 - 11 % Show Material materials with Níquel of 9 - 11 % |
Plomo | 0.02 % Show Material materials with Plomo of 0.02 % |
Zinc | 0.5 % Show Material materials with Zinc of 0.5 % |