General
Property | Value | Condition | Related Standards |
---|---|---|---|
Densidad | 2.77 g/cm³ Show Material materials with Densidad of 2.77 g/cm³ | O | |
2.78 g/cm³ Show Material materials with Densidad of 2.78 g/cm³ | O | AA Standards, ASTM B209, ASTM B210, ASTM B211, ASTM B241, ASTM B316 | |
3.0 g/cm³ Show Material materials with Densidad of 3.0 g/cm³ | O |
Mecánica
Property | Value | Condition | Related Standards | Comment |
---|---|---|---|---|
Bending Fatigue Strength | 90.0 MPa Show Material materials with Bending Fatigue Strength of 90.0 MPa | O | AA Standards | |
Coeficiente de Poisson | 0.33 [-] Show Material materials with Coeficiente de Poisson of 0.33 [-] | O | ||
Dureza Brinell | 47.0 [-] Show Material materials with Dureza Brinell of 47.0 [-] | O | AA Standards | |
Elongación | 10.0 % Show Material materials with Elongación of 10.0 % | O | AA Standards, ASTM B209, ASTM B241 | A100 |
12.0 % Show Material materials with Elongación of 12.0 % | O | AA Standards, ASTM B209, ASTM B241 | A50 | |
14.0 % Show Material materials with Elongación of 14.0 % | O | AA Standards, ASTM B211 | A100 | |
16.0 % Show Material materials with Elongación of 16.0 % | O | AA Standards, ASTM B211 | A50 | |
16.0 % Show Material materials with Elongación of 16.0 % | O | |||
20.0 % Show Material materials with Elongación of 20.0 % | O | AA Standards | A50 | |
20.0 % Show Material materials with Elongación of 20.0 % | O | AA Standards | A100 | |
20.0 % Show Material materials with Elongación of 20.0 % | O | |||
Límite elástico | 75.0 MPa Show Material materials with Límite elástico of 75.0 MPa | O | AA Standards | RP02 |
75.0 MPa Show Material materials with Límite elástico of 75.0 MPa | O | |||
95.0 MPa Show Material materials with Límite elástico of 95.0 MPa | O | AA Standards, ASTM B209 | RP02 | |
98.0 MPa Show Material materials with Límite elástico of 98.0 MPa | O | |||
100.0 MPa Show Material materials with Límite elástico of 100.0 MPa | O | AA Standards, ASTM B210 | RP02 | |
130.0 MPa Show Material materials with Límite elástico of 130.0 MPa | O | AA Standards, ASTM B241 | RP02 | |
Módulo de cizallamiento | 26.0 - 27.5 GPa Show Material materials with Módulo de cizallamiento of 26.0 - 27.5 GPa | Typical for Wrought 2000 Series Aluminium | ||
Módulo elástico | 72.4 GPa Show Material materials with Módulo elástico of 72.4 GPa | O | ||
73.0 GPa Show Material materials with Módulo elástico of 73.0 GPa | O | AA Standards, ASTM B209, ASTM B210, ASTM B211, ASTM B241, ASTM B316 | ||
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 2000 Series Aluminium | ||
Resistencia a la tracción | 185.0 MPa Show Material materials with Resistencia a la tracción of 185.0 MPa | O | AA Standards | |
190.0 MPa Show Material materials with Resistencia a la tracción of 190.0 MPa | O | |||
220.0 MPa Show Material materials with Resistencia a la tracción of 220.0 MPa | O | AA Standards, ASTM B209, ASTM B210 | ||
240.0 MPa Show Material materials with Resistencia a la tracción of 240.0 MPa | O | AA Standards, ASTM B211, ASTM B241, ASTM B316 |
Aplicaciones térmicas
Property | Temperature | Value | Condition | Related Standards |
---|---|---|---|---|
Calor específico | 870.0 J/(kg·K) Show Material materials with Calor específico of 870.0 J/(kg·K) | O | ||
875.0 J/(kg·K) Show Material materials with Calor específico of 875.0 J/(kg·K) | O | |||
Coeficiente de dilatación térmica | 2.29e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.29e-05 1/K | O | ||
2.3e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.3e-05 1/K | O | |||
20 °C | 2.3199999999999998e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.3199999999999998e-05 1/K | O | AA Standards, ASTM B209, ASTM B210, ASTM B211, ASTM B241, ASTM B316 | |
100 °C | 2.3199999999999998e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.3199999999999998e-05 1/K | O | AA Standards, ASTM B209, ASTM B210, ASTM B211, ASTM B241, ASTM B316 | |
Conductividad térmica | 120.0 W/(m·K) Show Material materials with Conductividad térmica of 120.0 W/(m·K) | O | ||
121.0 - 193.0 W/(m·K) Show Material materials with Conductividad térmica of 121.0 - 193.0 W/(m·K) | O | AA Standards, ASTM B209, ASTM B210, ASTM B211, ASTM B241, ASTM B316 | ||
190.0 W/(m·K) Show Material materials with Conductividad térmica of 190.0 W/(m·K) | O | |||
Temperatura de fusión | 500.0 °C Show Material materials with Temperatura de fusión of 500.0 °C | O | ||
505.0 - 635.0 °C Show Material materials with Temperatura de fusión of 505.0 - 635.0 °C | O | AA Standards, ASTM B209, ASTM B210, ASTM B211, ASTM B241, ASTM B316 |
Eléctrico
Property | Value | Condition | Related Standards | Comment |
---|---|---|---|---|
Conductividad eléctrica | 17000000.0 - 29000000.0 S/m Show Material materials with Conductividad eléctrica of 17000000.0 - 29000000.0 S/m | O | AA Standards, ASTM B209, ASTM B210, ASTM B211, ASTM B241, ASTM B316 | |
29000000 S/m Show Material materials with Conductividad eléctrica of 29000000 S/m | O | Typical/derived value | ||
Resistividad eléctrica | 3.4e-08 Ω·m Show Material materials with Resistividad eléctrica of 3.4e-08 Ω·m | O | Typical value | |
3.45e-08 - 5.88e-08 Ω·m Show Material materials with Resistividad eléctrica of 3.45e-08 - 5.88e-08 Ω·m | O | AA Standards, ASTM B209, ASTM B210, ASTM B211, ASTM B241, ASTM B316 | ||
Specific Electrical conductivity | 50.0 % IACS Show Material materials with Specific Electrical conductivity of 50.0 % IACS | O | Typical value |
Chemical properties
Property | Value | Condition | Related Standards |
---|---|---|---|
Aluminio | 90.7 - 94.7 % Show Material materials with Aluminio of 90.7 - 94.7 % | O | |
Circonio | 0.2 % Show Material materials with Circonio of 0.2 % | O | |
Cobre | 3.8 - 4.9 % Show Material materials with Cobre of 3.8 - 4.9 % | O | AA Standards, ASTM B209, ASTM B210, ASTM B211, ASTM B241, ASTM B316 |
Cromo | 0.1 % Show Material materials with Cromo of 0.1 % | O | AA Standards, ASTM B209, ASTM B210, ASTM B211, ASTM B241, ASTM B316 |
Hierro | 0.50 % Show Material materials with Hierro of 0.50 % | O | AA Standards, ASTM B209, ASTM B210, ASTM B211, ASTM B241, ASTM B316 |
0.5 % Show Material materials with Hierro of 0.5 % | O | ||
Magnesio | 1.2 - 1.8 % Show Material materials with Magnesio of 1.2 - 1.8 % | O | AA Standards, ASTM B209, ASTM B210, ASTM B211, ASTM B241, ASTM B316 |
Manganeso | 0.3 - 0.9 % Show Material materials with Manganeso of 0.3 - 0.9 % | O | AA Standards, ASTM B209, ASTM B210, ASTM B211, ASTM B241, ASTM B316 |
Otro | 0.15 % Show Material materials with Otro of 0.15 % | O | |
Silicona | 0.5 % Show Material materials with Silicona of 0.5 % | O | AA Standards, ASTM B209, ASTM B210, ASTM B211, ASTM B241, ASTM B316 |
Titanio | 0.15 % Show Material materials with Titanio of 0.15 % | O | AA Standards, ASTM B209, ASTM B210, ASTM B211, ASTM B241, ASTM B316 |
Zinc | 0.25 % Show Material materials with Zinc of 0.25 % | O | AA Standards, ASTM B209, ASTM B210, ASTM B211, ASTM B241, ASTM B316 |
Technological properties
Property | ||
---|---|---|
Brazing | general: no brazing is known or developed | |
Corrosion properties | Stress corrosion cracking: Betriebsschäden in Gebieten mit Zugspannungen quer zur Kornstruktur, Eingeschränkte Schäden an Laborproben (T4,T3, T351, T3510, T3511), d (T6, T861, T81, T851, T8510, T8511), general: sufficient, in principle it should be protected | |
General machinability | General: poor (O), good to acceptable | |
Workability | general (condition): poor(T4, T3, T351, T3510, T3511, T6), not suitable (T361, T861, T81, T851, T8510, T8511) |