General
Property | Value | Condition |
---|---|---|
Densidad | 4.4 g/cm³ Show Material materials with Densidad of 4.4 g/cm³ | Solution Treated |
Mecánica
Property | Value | Condition |
---|---|---|
Elongación | 8.7 % Show Material materials with Elongación of 8.7 % | Solution Treated |
Límite elástico | 1130.0 MPa Show Material materials with Límite elástico of 1130.0 MPa | Solution Treated |
Módulo elástico | 120.0 GPa Show Material materials with Módulo elástico of 120.0 GPa | Solution Treated |
Resistencia a la tracción | 1200.0 MPa Show Material materials with Resistencia a la tracción of 1200.0 MPa | Solution Treated |
Aplicaciones térmicas
Property | Value | Condition |
---|---|---|
Calor específico | 560.0 J/(kg·K) Show Material materials with Calor específico of 560.0 J/(kg·K) | Solution Treated |
Coeficiente de dilatación térmica | 8.9e-06 1/K Show Material materials with Coeficiente de dilatación térmica of 8.9e-06 1/K | Solution Treated |
Conductividad térmica | 6.8 W/(m·K) Show Material materials with Conductividad térmica of 6.8 W/(m·K) | Solution Treated |
Temperatura de fusión | 1650.0 °C Show Material materials with Temperatura de fusión of 1650.0 °C | Solution Treated |
Chemical properties
Property | Value | Condition |
---|---|---|
Aluminio | 5.5 - 6.8 % Show Material materials with Aluminio of 5.5 - 6.8 % | Solution Treated |
Carbono | 0.08 % Show Material materials with Carbono of 0.08 % | Solution Treated |
Hidrógeno | 0.015 % Show Material materials with Hidrógeno of 0.015 % | Solution Treated |
Hierro | 0.4 % Show Material materials with Hierro of 0.4 % | Solution Treated |
Itrio | 0.005 % Show Material materials with Itrio of 0.005 % | Solution Treated |
Nitrógeno | 0.05 % Show Material materials with Nitrógeno of 0.05 % | Solution Treated |
Otro | 0.4 % Show Material materials with Otro of 0.4 % | Solution Treated |
Oxígeno | 0.2 % Show Material materials with Oxígeno of 0.2 % | Solution Treated |
Titanio | 87.4 - 91.0 % Show Material materials with Titanio of 87.4 - 91.0 % | Solution Treated |
Vanadio | 3.5 - 4.5 % Show Material materials with Vanadio of 3.5 - 4.5 % | Solution Treated |