General
Property | Value | Condition |
---|---|---|
Densidad | 3.0 g/cm³ Show Material materials with Densidad of 3.0 g/cm³ | T4 |
Mecánica
Property | Value | Condition | Comment |
---|---|---|---|
Charpy impact energy, V-notch | 21.7 J Show Material materials with Charpy impact energy, V-notch of 21.7 J | T4 | |
Coeficiente de Poisson | 0.33 [-] Show Material materials with Coeficiente de Poisson of 0.33 [-] | T4 | |
Dureza Brinell | 95 [-] Show Material materials with Dureza Brinell of 95 [-] | T4 | 500 kg load, 10 mm b |
Elongación | 6.0 - 10.0 % Show Material materials with Elongación of 6.0 - 10.0 % | T4 | Sand cast, elongation in 50 mm |
8.5 % Show Material materials with Elongación of 8.5 % | T4 | ||
Límite elástico | 165.0 - 193.0 MPa Show Material materials with Límite elástico of 165.0 - 193.0 MPa | T4 | Sand cast, RP02 |
190.0 MPa Show Material materials with Límite elástico of 190.0 MPa | T4 | ||
Módulo de cizallamiento | 23.0 GPa Show Material materials with Módulo de cizallamiento of 23.0 GPa | T4 | |
Módulo elástico | 70.0 GPa Show Material materials with Módulo elástico of 70.0 GPa | T4 | |
71 GPa Show Material materials with Módulo elástico of 71 GPa | T4 | ||
Resistencia a la tracción | 275.0 - 345.0 MPa Show Material materials with Resistencia a la tracción of 275.0 - 345.0 MPa | T4 | Sand cast |
330.0 MPa Show Material materials with Resistencia a la tracción of 330.0 MPa | T4 | ||
Resistencia al cizallamiento | 255 MPa Show Material materials with Resistencia al cizallamiento of 255 MPa | T4 |
Aplicaciones térmicas
Property | Value | Condition |
---|---|---|
Calor específico | 920.0 J/(kg·K) Show Material materials with Calor específico of 920.0 J/(kg·K) | T4 |
Coeficiente de dilatación térmica | 2.1e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.1e-05 1/K | T4 |
Conductividad térmica | 120.0 W/(m·K) Show Material materials with Conductividad térmica of 120.0 W/(m·K) | T4 |
Temperatura de fusión | 570.0 °C Show Material materials with Temperatura de fusión of 570.0 °C | T4 |
Eléctrico
Property | Value | Condition | Comment |
---|---|---|---|
Conductividad eléctrica | 17400000 S/m Show Material materials with Conductividad eléctrica of 17400000 S/m | T4 | Typical/Derived values |
Resistividad eléctrica | 4.347826086956522e-08 - 6.25e-08 Ω·m Show Material materials with Resistividad eléctrica of 4.347826086956522e-08 - 6.25e-08 Ω·m | Typical for Cast 2xx.x Series Aluminium | |
Specific Electrical conductivity | 30 % IACS Show Material materials with Specific Electrical conductivity of 30 % IACS | T4 | Typical values |
Chemical properties
Property | Value | Condition |
---|---|---|
Aluminio | 93.3 - 95.3 % Show Material materials with Aluminio of 93.3 - 95.3 % | T4 |
Cobre | 4.2 - 5.0 % Show Material materials with Cobre of 4.2 - 5.0 % | T4 |
Estaño | 0.05 % Show Material materials with Estaño of 0.05 % | T4 |
Hierro | 0.15 % Show Material materials with Hierro of 0.15 % | T4 |
Magnesio | 0.15 - 0.35 % Show Material materials with Magnesio of 0.15 - 0.35 % | T4 |
Manganeso | 0.2 - 0.5 % Show Material materials with Manganeso of 0.2 - 0.5 % | T4 |
Níquel | 0.05 % Show Material materials with Níquel of 0.05 % | T4 |
Otro | 0.15 % Show Material materials with Otro of 0.15 % | T4 |
Silicona | 0.1 % Show Material materials with Silicona of 0.1 % | T4 |
Titanio | 0.15 - 0.3 % Show Material materials with Titanio of 0.15 - 0.3 % | T4 |
Zinc | 0.1 % Show Material materials with Zinc of 0.1 % | T4 |