General
Property | Value | Condition |
---|---|---|
Densidad | 3.0 g/cm³ Show Material materials with Densidad of 3.0 g/cm³ | T7 |
Mecánica
Property | Value | Condition | Comment |
---|---|---|---|
Coeficiente de Poisson | 0.33 [-] Show Material materials with Coeficiente de Poisson of 0.33 [-] | T7 | |
Dureza Brinell | 130 [-] Show Material materials with Dureza Brinell of 130 [-] | T7 | 500 kg load, 10 mm b |
Elongación | 12.0 % Show Material materials with Elongación of 12.0 % | T7 | |
Límite elástico | 350.0 MPa Show Material materials with Límite elástico of 350.0 MPa | T7 | |
Módulo de cizallamiento | 23.0 GPa Show Material materials with Módulo de cizallamiento of 23.0 GPa | T7 | |
Módulo elástico | 70.0 GPa Show Material materials with Módulo elástico of 70.0 GPa | T7 | |
71 GPa Show Material materials with Módulo elástico of 71 GPa | T7 | ||
Resistencia a la tracción | 440.0 MPa Show Material materials with Resistencia a la tracción of 440.0 MPa | T7 | |
Resistencia al cizallamiento | 260 MPa Show Material materials with Resistencia al cizallamiento of 260 MPa | T7 |
Aplicaciones térmicas
Property | Value | Condition |
---|---|---|
Calor específico | 920.0 J/(kg·K) Show Material materials with Calor específico of 920.0 J/(kg·K) | T7 |
Coeficiente de dilatación térmica | 2.1e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.1e-05 1/K | T7 |
Conductividad térmica | 120.0 W/(m·K) Show Material materials with Conductividad térmica of 120.0 W/(m·K) | T7 |
Temperatura de fusión | 570.0 °C Show Material materials with Temperatura de fusión of 570.0 °C | T7 |
Eléctrico
Property | Value | Condition | Comment |
---|---|---|---|
Conductividad eléctrica | 16000000.0 - 23000000.0 S/m Show Material materials with Conductividad eléctrica of 16000000.0 - 23000000.0 S/m | Typical for Cast 2xx.x Series Aluminium | |
Resistividad eléctrica | 5e-08 - 5.4e-08 Ω·m Show Material materials with Resistividad eléctrica of 5e-08 - 5.4e-08 Ω·m | T7 | Typical values |
Chemical properties
Property | Value | Condition |
---|---|---|
Aluminio | 93.3 - 95.3 % Show Material materials with Aluminio of 93.3 - 95.3 % | T7 |
Cobre | 4.2 - 5.0 % Show Material materials with Cobre of 4.2 - 5.0 % | T7 |
Estaño | 0.05 % Show Material materials with Estaño of 0.05 % | T7 |
Hierro | 0.15 % Show Material materials with Hierro of 0.15 % | T7 |
Magnesio | 0.15 - 0.35 % Show Material materials with Magnesio of 0.15 - 0.35 % | T7 |
Manganeso | 0.2 - 0.5 % Show Material materials with Manganeso of 0.2 - 0.5 % | T7 |
Níquel | 0.05 % Show Material materials with Níquel of 0.05 % | T7 |
Otro | 0.15 % Show Material materials with Otro of 0.15 % | T7 |
Silicona | 0.1 % Show Material materials with Silicona of 0.1 % | T7 |
Titanio | 0.15 - 0.3 % Show Material materials with Titanio of 0.15 - 0.3 % | T7 |
Zinc | 0.1 % Show Material materials with Zinc of 0.1 % | T7 |