General
Property | Value | Condition | Related Standards |
---|---|---|---|
Densidad | 2.84 g/cm³ Show Material materials with Densidad of 2.84 g/cm³ | T351 | AA Standards, ASTM B209 |
3.1 g/cm³ Show Material materials with Densidad of 3.1 g/cm³ | T351 |
Mecánica
Property | Value | Condition | Related Standards | Comment |
---|---|---|---|---|
Coeficiente de Poisson | 0.33 [-] Show Material materials with Coeficiente de Poisson of 0.33 [-] | Typical for Wrought 2000 Series Aluminium | ||
Elongación | 7.0 % Show Material materials with Elongación of 7.0 % | T351 | AA Standards, ASTM B209 | A100 |
8.0 % Show Material materials with Elongación of 8.0 % | T351 | AA Standards, ASTM B209 | A100 | |
9.0 % Show Material materials with Elongación of 9.0 % | T351 | AA Standards, ASTM B209 | A100 | |
10.0 % Show Material materials with Elongación of 10.0 % | T351 | AA Standards, ASTM B209 | A50 | |
14.0 % Show Material materials with Elongación of 14.0 % | T351 | |||
17.0 % Show Material materials with Elongación of 17.0 % | T351 | AA Standards | A50 | |
Límite elástico | 170.0 MPa Show Material materials with Límite elástico of 170.0 MPa | T351 | AA Standards, ASTM B209 | RP02 |
180.0 MPa Show Material materials with Límite elástico of 180.0 MPa | T351 | AA Standards, ASTM B209 | RP02 | |
185.0 MPa Show Material materials with Límite elástico of 185.0 MPa | T351 | AA Standards, ASTM B209 | RP02 | |
195.0 MPa Show Material materials with Límite elástico of 195.0 MPa | T351 | AA Standards, ASTM B209 | RP02 | |
230.0 MPa Show Material materials with Límite elástico of 230.0 MPa | T351 | |||
250.0 MPa Show Material materials with Límite elástico of 250.0 MPa | T351 | AA Standards | RP02 | |
Módulo de cizallamiento | 26.0 - 27.5 GPa Show Material materials with Módulo de cizallamiento of 26.0 - 27.5 GPa | Typical for Wrought 2000 Series Aluminium | ||
Módulo elástico | 73.0 GPa Show Material materials with Módulo elástico of 73.0 GPa | T351 | AA Standards, ASTM B209 | |
74.0 GPa Show Material materials with Módulo elástico of 74.0 GPa | T351 | |||
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 2000 Series Aluminium | ||
Resistencia a la tracción | 270.0 MPa Show Material materials with Resistencia a la tracción of 270.0 MPa | T351 | AA Standards, ASTM B209 | |
275.0 MPa Show Material materials with Resistencia a la tracción of 275.0 MPa | T351 | AA Standards, ASTM B209 | ||
290.0 MPa Show Material materials with Resistencia a la tracción of 290.0 MPa | T351 | AA Standards, ASTM B209 | ||
305.0 MPa Show Material materials with Resistencia a la tracción of 305.0 MPa | T351 | AA Standards, ASTM B209 | ||
315.0 MPa Show Material materials with Resistencia a la tracción of 315.0 MPa | T351 | AA Standards, ASTM B209 | ||
350.0 MPa Show Material materials with Resistencia a la tracción of 350.0 MPa | T351 | |||
360.0 MPa Show Material materials with Resistencia a la tracción of 360.0 MPa | T351 | AA Standards |
Aplicaciones térmicas
Property | Temperature | Value | Condition | Related Standards |
---|---|---|---|---|
Calor específico | 860.0 J/(kg·K) Show Material materials with Calor específico of 860.0 J/(kg·K) | T351 | ||
Coeficiente de dilatación térmica | 2.2e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.2e-05 1/K | T351 | ||
20 °C | 2.23e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.23e-05 1/K | T351 | AA Standards, ASTM B209 | |
100 °C | 2.23e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.23e-05 1/K | T351 | AA Standards, ASTM B209 | |
Conductividad térmica | 113.0 - 172.0 W/(m·K) Show Material materials with Conductividad térmica of 113.0 - 172.0 W/(m·K) | T351 | AA Standards, ASTM B209 | |
140.0 W/(m·K) Show Material materials with Conductividad térmica of 140.0 W/(m·K) | T351 | |||
Temperatura de fusión | 540.0 °C Show Material materials with Temperatura de fusión of 540.0 °C | T351 | ||
545.0 - 645.0 °C Show Material materials with Temperatura de fusión of 545.0 - 645.0 °C | T351 | AA Standards, ASTM B209 |
Eléctrico
Property | Value | Condition | Related Standards | Comment |
---|---|---|---|---|
Conductividad eléctrica | 16000000.0 - 26000000.0 S/m Show Material materials with Conductividad eléctrica of 16000000.0 - 26000000.0 S/m | T351 | AA Standards, ASTM B209 | |
16000000 S/m Show Material materials with Conductividad eléctrica of 16000000 S/m | T351 | Typical/derived value | ||
Resistividad eléctrica | 3.85e-08 - 6.25e-08 Ω·m Show Material materials with Resistividad eléctrica of 3.85e-08 - 6.25e-08 Ω·m | T351 | AA Standards, ASTM B209 | |
5.7e-08 Ω·m Show Material materials with Resistividad eléctrica of 5.7e-08 Ω·m | T351 | Typical value | ||
Specific Electrical conductivity | 28.0 % IACS Show Material materials with Specific Electrical conductivity of 28.0 % IACS | T351 | Typical value |
Chemical properties
Property | Value | Condition | Related Standards |
---|---|---|---|
Aluminio | 91.5 - 93.8 % Show Material materials with Aluminio of 91.5 - 93.8 % | T351 | |
Circonio | 0.1 - 0.25 % Show Material materials with Circonio of 0.1 - 0.25 % | T351 | AA Standards, ASTM B209 |
Cobre | 5.8 - 6.8 % Show Material materials with Cobre of 5.8 - 6.8 % | T351 | AA Standards, ASTM B209 |
Hierro | 0.30 % Show Material materials with Hierro of 0.30 % | T351 | AA Standards, ASTM B209 |
0.3 % Show Material materials with Hierro of 0.3 % | T351 | ||
Magnesio | 0.02 % Show Material materials with Magnesio of 0.02 % | T351 | AA Standards, ASTM B209 |
Manganeso | 0.2 - 0.4 % Show Material materials with Manganeso of 0.2 - 0.4 % | T351 | AA Standards, ASTM B209 |
Otro | 0.15 % Show Material materials with Otro of 0.15 % | T351 | |
Silicona | 0.2 % Show Material materials with Silicona of 0.2 % | T351 | AA Standards, ASTM B209 |
Titanio | 0.02 - 0.1 % Show Material materials with Titanio of 0.02 - 0.1 % | T351 | AA Standards, ASTM B209 |
Vanadio | 0.05 - 0.15 % Show Material materials with Vanadio of 0.05 - 0.15 % | T351 | AA Standards, ASTM B209 |
Zinc | 0.1 % Show Material materials with Zinc of 0.1 % | T351 | AA Standards, ASTM B209 |
Technological properties
Property | ||
---|---|---|
Brazing | general: no brazing is known or developed | |
Corrosion properties | Stress corrosion cracking: Betriebsschäden in Gebieten mit Zugspannungen quer zur Kornstruktur, Eingeschränkte Schäden an Laborproben (T31, T351, T3510, T3511, T37), kein Schadensfall im Betrieb, eingeschränkte Schäden bei den Labortests (T81, T851, T8510, T8511), general: sufficient, in principle it should be protected | |
General machinability | General: good to acceptable | |
Workability | general (condition): poor(T31, T351, T3510, T3511), not suitable (T37, T81, T851, T8510, T8511, T87) |