General
Property | Value | Condition | Related Standards |
---|---|---|---|
Densidad | 2.84 g/cm³ Show Material materials with Densidad of 2.84 g/cm³ | T6 | AA Standards, ASTM B247, ASTM B316 |
3.1 g/cm³ Show Material materials with Densidad of 3.1 g/cm³ | T6 |
Mecánica
Property | Value | Condition | Related Standards | Comment |
---|---|---|---|---|
Coeficiente de Poisson | 0.33 [-] Show Material materials with Coeficiente de Poisson of 0.33 [-] | Typical for Wrought 2000 Series Aluminium | ||
Elongación | 1.0 % Show Material materials with Elongación of 1.0 % | T6 | AA Standards, ASTM B247 | A100 |
2.0 % Show Material materials with Elongación of 2.0 % | T6 | AA Standards, ASTM B247 | A50 | |
3.0 % Show Material materials with Elongación of 3.0 % | T6 | AA Standards, ASTM B247 | A100 | |
4.0 % Show Material materials with Elongación of 4.0 % | T6 | AA Standards, ASTM B247 | A50 | |
5.0 % Show Material materials with Elongación of 5.0 % | T6 | AA Standards, ASTM B247, ASTM B316 | A100 | |
5.5 % Show Material materials with Elongación of 5.5 % | T6 | |||
6.0 % Show Material materials with Elongación of 6.0 % | T6 | AA Standards, ASTM B247 | A50 | |
7.0 % Show Material materials with Elongación of 7.0 % | T6 | AA Standards, ASTM B247 | A100 | |
8.0 % Show Material materials with Elongación of 8.0 % | T6 | AA Standards, ASTM B247 | A50 | |
Límite elástico | 240.0 MPa Show Material materials with Límite elástico of 240.0 MPa | T6 | AA Standards, ASTM B247, ASTM B316 | RP02 |
250.0 MPa Show Material materials with Límite elástico of 250.0 MPa | T6 | AA Standards, ASTM B247 | RP02 | |
255.0 MPa Show Material materials with Límite elástico of 255.0 MPa | T6 | AA Standards, ASTM B247 | RP02 | |
260.0 MPa Show Material materials with Límite elástico of 260.0 MPa | T6 | AA Standards, ASTM B247 | RP02 | |
275.0 MPa Show Material materials with Límite elástico of 275.0 MPa | T6 | AA Standards, ASTM B247 | RP02 | |
280.0 MPa Show Material materials with Límite elástico of 280.0 MPa | T6 | |||
Módulo de cizallamiento | 26.0 - 27.5 GPa Show Material materials with Módulo de cizallamiento of 26.0 - 27.5 GPa | Typical for Wrought 2000 Series Aluminium | ||
Módulo elástico | 73.0 GPa Show Material materials with Módulo elástico of 73.0 GPa | T6 | AA Standards, ASTM B247, ASTM B316 | |
74.0 GPa Show Material materials with Módulo elástico of 74.0 GPa | T6 | |||
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 2000 Series Aluminium | ||
Resistencia a la tracción | 365.0 MPa Show Material materials with Resistencia a la tracción of 365.0 MPa | T6 | AA Standards, ASTM B247 | |
380.0 MPa Show Material materials with Resistencia a la tracción of 380.0 MPa | T6 | AA Standards, ASTM B247, ASTM B316 | ||
385.0 MPa Show Material materials with Resistencia a la tracción of 385.0 MPa | T6 | AA Standards, ASTM B247 | ||
400.0 MPa Show Material materials with Resistencia a la tracción of 400.0 MPa | T6 | AA Standards, ASTM B247 | ||
430.0 MPa Show Material materials with Resistencia a la tracción of 430.0 MPa | T6 |
Aplicaciones térmicas
Property | Temperature | Value | Condition | Related Standards |
---|---|---|---|---|
Calor específico | 860.0 J/(kg·K) Show Material materials with Calor específico of 860.0 J/(kg·K) | T6 | ||
Coeficiente de dilatación térmica | 2.2e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.2e-05 1/K | T6 | ||
20 °C | 2.23e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.23e-05 1/K | T6 | AA Standards, ASTM B247, ASTM B316 | |
100 °C | 2.23e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.23e-05 1/K | T6 | AA Standards, ASTM B247, ASTM B316 | |
Conductividad térmica | 113.0 - 172.0 W/(m·K) Show Material materials with Conductividad térmica of 113.0 - 172.0 W/(m·K) | T6 | AA Standards, ASTM B247, ASTM B316 | |
120.0 W/(m·K) Show Material materials with Conductividad térmica of 120.0 W/(m·K) | T6 | |||
Temperatura de fusión | 540.0 °C Show Material materials with Temperatura de fusión of 540.0 °C | T6 | ||
545.0 - 645.0 °C Show Material materials with Temperatura de fusión of 545.0 - 645.0 °C | T6 | AA Standards, ASTM B247, ASTM B316 |
Eléctrico
Property | Value | Condition | Related Standards | Comment |
---|---|---|---|---|
Conductividad eléctrica | 16000000.0 - 26000000.0 S/m Show Material materials with Conductividad eléctrica of 16000000.0 - 26000000.0 S/m | T6 | AA Standards, ASTM B247, ASTM B316 | |
17000000 S/m Show Material materials with Conductividad eléctrica of 17000000 S/m | T6 | Typical value | ||
Resistividad eléctrica | 3.85e-08 - 6.25e-08 Ω·m Show Material materials with Resistividad eléctrica of 3.85e-08 - 6.25e-08 Ω·m | T6 | AA Standards, ASTM B247, ASTM B316 | |
5.8999999999999986e-08 Ω·m Show Material materials with Resistividad eléctrica of 5.8999999999999986e-08 Ω·m | T6 | Typical value | ||
Specific Electrical conductivity | 29.0 % IACS Show Material materials with Specific Electrical conductivity of 29.0 % IACS | T6 | Typical/Derived value |
Chemical properties
Property | Value | Condition | Related Standards |
---|---|---|---|
Aluminio | 91.5 - 93.8 % Show Material materials with Aluminio of 91.5 - 93.8 % | T6 | |
Circonio | 0.1 - 0.25 % Show Material materials with Circonio of 0.1 - 0.25 % | T6 | AA Standards, ASTM B247, ASTM B316 |
Cobre | 5.8 - 6.8 % Show Material materials with Cobre of 5.8 - 6.8 % | T6 | AA Standards, ASTM B247, ASTM B316 |
Hierro | 0.30 % Show Material materials with Hierro of 0.30 % | T6 | AA Standards, ASTM B247, ASTM B316 |
0.3 % Show Material materials with Hierro of 0.3 % | T6 | ||
Magnesio | 0.02 % Show Material materials with Magnesio of 0.02 % | T6 | AA Standards, ASTM B247, ASTM B316 |
Manganeso | 0.2 - 0.4 % Show Material materials with Manganeso of 0.2 - 0.4 % | T6 | AA Standards, ASTM B247, ASTM B316 |
Otro | 0.15 % Show Material materials with Otro of 0.15 % | T6 | |
Silicona | 0.2 % Show Material materials with Silicona of 0.2 % | T6 | AA Standards, ASTM B247, ASTM B316 |
Titanio | 0.02 - 0.1 % Show Material materials with Titanio of 0.02 - 0.1 % | T6 | AA Standards, ASTM B247, ASTM B316 |
Vanadio | 0.05 - 0.15 % Show Material materials with Vanadio of 0.05 - 0.15 % | T6 | AA Standards, ASTM B247, ASTM B316 |
Zinc | 0.1 % Show Material materials with Zinc of 0.1 % | T6 | AA Standards, ASTM B247, ASTM B316 |
Technological properties
Property | ||
---|---|---|
Brazing | general: no brazing is known or developed | |
Corrosion properties | Stress corrosion cracking: Betriebsschäden in Gebieten mit Zugspannungen quer zur Kornstruktur, Eingeschränkte Schäden an Laborproben (T31, T351, T3510, T3511, T37), kein Schadensfall im Betrieb, eingeschränkte Schäden bei den Labortests (T81, T851, T8510, T8511), general: sufficient, in principle it should be protected | |
General machinability | General: good to acceptable | |
Workability | general (condition): poor(T31, T351, T3510, T3511), not suitable (T37, T81, T851, T8510, T8511, T87) |